CA1179440A - Polymer/polyols, methods for making same and polyurethanes based thereon - Google Patents

Polymer/polyols, methods for making same and polyurethanes based thereon

Info

Publication number
CA1179440A
CA1179440A CA000412105A CA412105A CA1179440A CA 1179440 A CA1179440 A CA 1179440A CA 000412105 A CA000412105 A CA 000412105A CA 412105 A CA412105 A CA 412105A CA 1179440 A CA1179440 A CA 1179440A
Authority
CA
Canada
Prior art keywords
polyol
polymer
polyols
coupled
styrene
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
CA000412105A
Other languages
French (fr)
Inventor
Russell Van Cleve
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Union Carbide Corp
Original Assignee
Union Carbide Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Union Carbide Corp filed Critical Union Carbide Corp
Priority to CA000443577A priority Critical patent/CA1197046A/en
Application granted granted Critical
Publication of CA1179440A publication Critical patent/CA1179440A/en
Expired legal-status Critical Current

Abstract

ABSTRACT OF THE DISCLOSURE
This invention relates to normally liquid, stable polymer/polyol compositions formed by polymerizing, in the presence of a free radical catalyst, an ethylenically unsaturated monomer or monomers dissolved or dispersed in a polyol mixture including a coupled polyol consisting of the reaction product of a polyol having a functionality in excess of 2 reacted with a polyisocyanate in such proportion that the ratio of hydroxyl groups to isocyanato groups is greater than 1. In one embodiment, the coupled polyol is made in situ in the base polyol by addition thereto of the required amount of the polyisocyanate. The novel polymer/polyol compositions are convertible to polyurethane foams and elastomers.

Description

~1~7~

, BACKGROUND OF THE INVENTION
This invention relates to polymer/polyol compositions and to polyurethanes utilizing such compositions.
Polymer/polyol compositions suitable for use in producing polyurethane foams, elastomers and the like are known materials. Such compositions can be produced by polymerizing one or more ethylenically unsaturated monomers dissolved or dispersed in a polyol in the presence of a free radical catalyst. These polymer/polyol compositions have the valuable property of imparting to, for example, polyurethane foams and elastomers produced therefrom, higher load-bearing properties than are provided by the corresponding unmodified polyols.
There are a number of prior disclosures relating to production of polymer/polyol compositions. The basic patents in the field are Stamberger Re. 28,715 (reissue of U.S. 3,383,351) and Re. 29,118 (reissue of U.S. 3,304,273). Other prior disclosures include: 8ritish Patent No.
1,126,025; Scharf et al. Canadian Patent No.
735,010; Kuryla Canadian Patent No. 785~835; Pizzini et al. U.S. 3,652,639; Pizzini et al. Re. 29,014 2S (reissue of U.S. 3,823,201); Pattong Jr., et al.
U.S. 3,950,317; Ramlow et al. U.S. 3,953,393; DeWald U.S. 3,6559553; Fabris et al. U.S. 3,850,861; Priest et al. U.S. 4,208,314; Simroth U.S. 4,104,236i Shah U.S. 4,148,840; Shah U.S. 4,119,586; Shook et al.
U.S. 4,172,825; Drake et al. U.S. 4,198,488; Preston et al. U.S. 4,198,488; Japanese Patent No.
48-101494; and Japanese Patent No. 52-80919/75.

'~

. .
- 2 -The polymer/polyol compositions that found initial commercial acceptance were primarily compositions produced using acrylonitrile. Such compositions were somewhat higher in viscosity than desired in some applications. Further, such S compositions were at least primarily used commercially in producing foams under conditions such that the heat generated during foaming is readily dissipated (e.g. - the foams have a relatively thin cross-section) or under conditions such that relatively little heat is generated during foaming. When polyurethane foams were produced under conditions such that the heat generated during foaming was not readily dissipated, severe foam scorching usually resulted. Later, polymer/polyol compositions produced from acrylonitrile-methylmethacrylate monomer mixtures were commercialized and were convertible to polyurethane foams having reduced scorch.
More recently, polymer/polyol compositions produced from acrylonitrile-styrene monomer mixtures have been used commercially. Use of low ratios of acrylonitrile-to-styrene in the monomer mixture affords polymer/polyols that do not give rise to a scorch problem. But it is increasingly difficu1t to make satisfactorily stable polymer/polyols as the ratio of acrylonitrile to styrene is reduced to the desired levels.
The development of sophisticated, high speed and large volume equipment, machines and systems for handling, mixing and reacting polyurethane-forming ingredients has created the need for highly stable polymer/polyols. At one time, there was not much concern for the seediness, . ., ViscQsity or filterabi1ity of polymer/polyols in actual commercial practice. However, the state of the art of polyurethane production has now advanred to the point where these considerations are very important in many applications. There is now much concern with filterability, seediness, and viscosity; and polymer/polyols must meet certain minimum requirements in order to be capable of being processed in the sophisticated foam equipment now used. Typically, the prime requirement is that the - polymer/polyols possess sufficiently small particles so that filters, pumps and the like do not become plugged or fouled in relatively short periods of time.
While somewhat simplified, the commercial processability of a particular polymer/polyol comes down to its viscosity and stability against phase separation. Lower viscosities are of substantial practical and economic significance due to the ease of pumping and metering as well as ease of mixing during the formation of polyurethanes. Stability is a prime consideration in insuring that the polymer/polyols can be processed in commercial production equipment without the necessity of additional mixing to insure homogeneity.
In addition to the monomer ratio in acrylonitrile-styrene polymer/polyols, other recognized factors that affect product stability include polyol molecular weight and polymer content.
In producing polymer/polyols for use in certain polyurethane ela,tomer applications, relatively low molecular weight polyols are typically utilized to provide the requisite product stiffness. However, it has been found that it is ~2895 '7~

. .

increasingly difficlllt to make satisfactorily stable polymertpolyols as the molecular weight of the polyol is decreased.
Still other applications could desirably utilize polyurethane foams and elastomers with even higher load-bearing capacities than can be currently provided using avaiiable polymer/polyols. However, it has been found that it is increasingly difficult to make satisfactorily stable polymer/polyols as the amount of polymer is increased.
U.S. Patent No. 4,208,314 to Priest et al.
discloses low viscosity polymertpolyols made from acrylonitrile-styrene monomer mixtures. These polymertpolyols can be converted to low density, water blown polyurethane foams having reduced scorch, especially when the acrylonitrile to styrene ratio is relatively low. The Priest et al. patent also provides a process for making polymer/polyols whereby the particulate nature of the product is considerably improved, compared to polymer/polyols prepared by prior processes. Using prior procedures, such as the one disclosed in Canadian Patent No. 735,010, polymertpolyols formed from such monomer mixtures usual1y contained excessive amounts of large granules. The improved process provided by Priest et al. includes, in genera1, maintaining a low monomer concentration throughout the reaction mixture during the polymerization.
U.S. Patent No. 4,104,236 to Simroth discloses a substantial further improvement in forming polymertpolyols made from acrylonitrile-styrene monomer mixtures, which enables selection of the polymer content to provide a polymertpolyol having satisfactory stability when a polyol of given ~7~

molecular weight and a monomer mixture having a ratio of acrylonitrile to styrene within a certain range are used. The Simroth patent also highlights the fact that satisfactory product stability is not ob-tained when many combinations of otherwise desirable composition parameters are used.
U.S. Patent No. 4,172,~25 to Shook et al.
discloses further improvements in the formation of polymer/polyols. As discussed therein, polymer/polyol compositions exhibiting outstanding properties can be made by utilizing a specific type of peroxide catalyst, namely t-alkyl peroxyester cataly~ts. By utilizing this specific type of catalyst, polymer/polyols can be produced on a commercial basis which have outstanding properties, lS such as filterability in processing, yet which allow either the polymer or the styrene content to be increased. Also, polymer/polyols can be produced on a commercial scale with polyols having a molecular weight lower than had been used prior to this invention.
A further improvement in the formation of polymer/polyols is provided by U.S. Patent No.
4,148,840 to Shah, which discloses a process ~or producing highly stab1e and filterable polymer/polyol compositions by polymerizing the monomer or monomers in situ in a polyol mixture that includes a minor amount of preformed polymer/polyol.
Yet another improvement is disclosed in U.S. Patent No. 49119,586 to Shah, which discloses a 3Q process for producing highly stable polymer/polyol compositions by polymerizing the monomer or monomers in situ in a polyol mixture that includes a major amount of a low molecular weight polyol and a minor amount of high molecular weight polyol.

...

U.S. Patent 4,242,249 to VanCleve et al.
discloses yet another approach to producing stable polymer/polyols in cases where the composition parameters are such that conventional processes would not usually afford a stable product. In the process disclosed by this patent, the monomer mixture is polymerized in a polyol that contains a minor amount of a preformed stabilizer that is tailored to the monomer mixture usedO The stabilizer is a copolymer comprised of an anchor por~ion that is a polymer of the monomer mixture, and a solvatable portion consisting of a propylene oxide polymer having a number average molecular weight of at least about 800.
It has been recognized that the stability of polymer/polyols requires the presence of a minor amount of a graft or addition copolymer which is formed in situ from the polymer and polyol. Some prior approaches have thus been directed to incorporation of amounts of unsaturation to the polyol in addition to that inherently present in the polyoxyalkylene polyols typically used in forming polymer/polyols in the belief that improved stability will result due to an increased amount of an addition copolymer stabilizer expected to be formed. U.S. Patent Nos. 3,652,639, 3,823,201, and
3,850,861, British Patent No. 1,126,025, and Japanese Patents Nos. 52-80919 and 48-101494 all utilize this approach.
U.S. Patent No. 3,850,861 thus discloses the in situ polymerization of ethylenically unsaturated monomers in an unsaturated polyol.
Suitable polyols are prepared by using an ethylenically unsaturated po1yhydric initiator to form a polyalkylene oxide. The examples set forth include dibasic acids or their derivatives, such as ma1eic acid. The polyol polymerization medium contains one mole of unsaturation per mole of polyol.
U.S. Patent No. 3,652,639 likewise ; discloses the in situ polymerization of ethylenically unsaturated monomers in an ethylenically unsaturated polyol medium. The unsaturated polysls of this patent are produced in a manner similar to those of U.S~ Patent No. 3,823,201, as will be discussed hereinafter, except that the level of unsaturation is higher, being on the order of l to 3 moles of unsaturation per mole of polyol.
U.S. Patent No. 3,823,201 discloses a method of preparing a polymer/polyol by the in situ polymerization of ethylen;cally unsaturated monomers in a polyol having from 0.1 to 0.7 mole of unsaturation per mole of polyol. Unsaturation at the levels set forth in the U.S. Patent No.
3,652,63~ patent were indicated as imparting unnecessarily high viscosities to the resulting polymer/polyols. The unsaturation level that is added can be introduced into the polyol by, for example, reacting it with an ethylenically unsaturated compound that is capable of adding to the polyol by reaction with the hydroxyl group, such as maleic anhydride. The polymer/polyols disclosed in U.S. Patent No. 3,823,201 are asser~ed to be highly stable due to the presence of the stabilizing species which is formed via the grafting of vinyl polymer chain segments to the unsaturated polyol molecules. Certain improvements in polyurethanes using such polymer/polyols are likewise asserted.
More particularly, it is stated that such ~:~'7~
:
~ 8 -polymer/polyols are surprisingly superior to those prepared from polyols having high unsaturation in regard to their low viscosities. It is further stated that polyurethane foams prepared from these ~raft copolymers exhibit superior load-bearing properties.
British Patent No. 1,126,025 discloses in situ polymerization of ethylenically unsaturated rnonomers in a polyol having a molecular weight from 250 to 10,000, preferably from 300 to 7,000, and containing at-least 0.7 double bonds per molecule.
It is stated that suitable unsaturated polyols can be made by including unsaturated compounds such as unsaturated polyhydric alcohols, polycarboxylic acids, or epoxides in the reaction mixture when the polyol is formed, but that it is preferred to introduce the unsaturation by reacting a preformed polyol with an unsaturated epox;de, e.g., allyl glycidyl ether.
Japanese Patent No. 52-80919 discloses products that are said to be useful in preparation of polyurethanes which are produced by polymerizing unsaturated polyether-esters, or copolymerizing an unsaturated polyether-ester with a vinyl monomer.
The unsaturated polyether-ester is prepared by reacting a polyol having a molecular weight of 1,000 to 30,000 with d mixture of saturated and unsaturated dicarboxylic acids. It is stated that the mole ratio of saturated dicarboxylic acid to unsaturated dicarboxylic acid should be from 95tS to 50/50 to control polymerization. In the Examples, the products are described as being very homogeneous and stable.

Japanese Patent No. 48-101494 discloses in situ polymerization of ethylenically unsaturated monomers in modified polyether polyols obtained by reacting a polyether polyol first with an unsaturated dicarboxylic acid anhydride in an amount more than 0.2 mole per mole of polyol, and then with an epoxy compound, preferably an alkylene oxide, in an amount of preferably 1.1 to 1.5 moles per mole of unsaturated dicarboxylic acid anhydride.
A further approach to production of polymer/polyols is disclosed in U.S. Patent No.
4,198,488 to Drake et al. In the process disclosed in this patent, the monomer mixture that is polymerized in the polyol includes a minor amount of an ethylenically unsaturated dicarboxylic acid anhydride. It was theorized that some graft copolymer is produced when a portion of the dicarboxylic acid anhydride units that have polymerized into the polymer undergo a reaction with the hydroxyl groups of the polyol. And it was further theorized that the graft copolymer formed in this way acts as a stabilizer for the polymer dispersion.
While many of the above techniques have provided improved and beneficial results, there are certain cases where none of these techniques have provided products which were entirely satisfactory.
Thus, for example, in some situations, the use of the blended base polyol approach results in an undue lowering of the hydroxyl number of the blend with a resultant adverse effect upon foam performance.
Other approaches, while generally satisfactory, are too expensive for many commercial applications, too complicated, result in color and odor problems or - lo require foam reformulations which can create undue difficulties.
It is highly desirable for low density slab stock foam applications to be able to provide virtually scorch-free products. This can be accomplished at foam densities of about 2.5 pounds per cubic foot or so It may also be possible with existing technology to provide foams with scorch-free characteristics at even lower densities; but, typically, the technology used either requires an economic penalty or results in less than satisfactory ~oam charaeteristics. There thus remains the need to provide techniques capable of producing, without substantial economic penalty, virtually scorch-free slab stock foams at ever decreasing densities (viz.-1.75 pounds per cubic foot or less) while maintaining satisfactory load-bearing and other foam properties.
Further, some foam applications require quite rigorous combustibility resistance. It is quite difficult with existing polymer/polyol technology to provide foams from vinyl monomer systems which meet such requirements. There thus remains an unfilled need to provide technology which can utilize vinyl monomer systems, yet satisfy these rigorous combustibility standards.
There has also been considerable development directed towards making and utilizing various polyols modified by what has been sometimes described as coupling agentsO Prior patents directed to such coupled polyols include: U.S.
Patent Nos. 2,946,767; 3,054,778; 3,963,818;
4,018,815; 4,045,474; 4,061,614; 4,061,684;
4,072,704 and 4,113,785.

Coupled polyols are utilized for many app1ications. For example, U.S. Patent No.
4,072,704 provides products useful as sur~actants made from individual blocks of polymers and copolymers of alkylene oxides by reacting these with bifunctional compounds. U.S. Patent No. 4,061,684 suggests the preparation of highly branched polyether polyols of high molecular weight by coupling an alkoxylatecl polyglycerol by reacting the sodium alcoholate of the oxyalkylated polyglycerol with, for example, a dibenzene sulfo-ester of a diol containing 2 to 6 carbon atoms. The resulting products are viscous, resinous materials, suitable for use as hydrophilic, water-swellable gels, and the like. U.S. Patent No. 4,113,785 concerns the preparation of polyoxyalkylene polyols by reacting polyether bis-alcoholates with selected bis-epoxides, to obtain products of higher molecular weight than can be prepared using a direct oxyalkylation reaction.
Still further, the utilization of various isocyanates as coupling agents for various polyol, or polyol-type materials, has been suggested. U.S.
Patent No~ 2,946,767 thus suggests the reaction of a polyisocyanate, especially a diisocyanate, with an addition product having a molecular weight of at least 1000 of an alkylene oxide, especially ethylene oxide, with a compound which contains at least 8 carbon atoms and contains only one hydrogen atom capable of reacting with an alkylene oxide, e.g. - a monoalcohol such as dodecanol~ The reaction products are surface-active and are stated to be valuable assistants for the production of dispersed systems, such as emulsions or suspensions.

~L~7~ 3 - -I

U.S. Patent No. 3,054,778 suggests the reaction of polyoxyethylene glycol, or a polyoxyalkylene glycol that is water~soluble and consists predominantly of oxyethylene groups, ~ith an organic diisocyanate in proportions and under conditions such that a substantially linear, water-soluble, film forming, orientable, polyglycol-polyurethane resin having high tensile strength and elongation is produced. The resins are useful as warp-sizing agents, flocculating agents in aqueous media and for the production of films and fibers.
U.S. Patent No. 3,963,681 discloses elastomer compositions prepared by using polyfunctional isocyanate, curing agent and ~ertain polyethers having a weight average molecular weight within the range of 1000 to less than 4,500. As the polyether, it is suggested that a pre-extended polyether may be used, which is prepared by subjecting a low molecular weight polyether to reaction with a diisocyanate or by subjecting a diol compound to reaction with a diisocyanate prepolymer of polyether.
Despite all of these prior efforts, no one has suggested the utilization per se of an isocyanate-coupled polyol to provide polymer/polyols or polyurethanes utilizing such polymer/polyols.
Indeed, the only known prior use of such coupled polyols in polymer/polyols is described in U.S.
Patent No. 4,242,249 to VanCleve et al., previously described, wherein one technique for forming the preformed stabilizer consisting of an anchor portion and a solvatable portion employs a solvatable portion which is the reaction product of a propylene oxide material with toluene diisocyanate. The ~ 3 I

resulting solvatable portion is then reacted with the monomer or monomers forming the anchor portion to provide the preformed stabilizer. It is stated that it is preferred that the propylene oxide material be monofunctional, although difunctional materials are satisfactory. The use of tri- or higher functionality materials, it is noted, should be avoided as extensive cross-linking has been found to occur.
It is accordingly an object of the present invention to provide polymer/polyols characterized by satisfactory stability which could not be readily made by prior techniques.
A further object provides a process for making such polymer/polyols that is relatively straight forward and does not require significant economic penalties as compared with currently known techniques.
Yet another and more specific object of this invention is to provide a technique for preparing such polymer/polyols capable of conversion to polyurethanes without imparting thereto undesirable effects upon the physical properties.
A still further object of the present invention is to provide a virtually scorch-free, relatively low density, polyurethane slab-stock ~oam made from a vinyl polymer, polymer/polyol.
Other objects of this invention will be apparent from the description set forth hereinafter.

SUMMARY OF ThE INVENTION
The present invention is based on the discovery that polymer/polyols with satisfactory s.ability and other characteristics can be provided by utilizing a polyisocyanate-coupled polyol. This invention thus provides a normally liquid, stable polymer/polyol composition formed by polymerizing, in the presence of a free radical catalyst, (1) from about 10 to about 50 weight percent of a mixture of acrylonitrile and styrene in a weight ratio, respectively, of from about 80:20 to about 20:80, dissolved or dispersed in (2) from about 50 to about 90 weight percent of a polyol mixture consisting of (a) a base polyol having a number average molecular weight of at least about 500 and (b) a coupled polyol consisting essentially of the reaction product of a polyol having a functionality in excess of 2 reacted with a polyisocyanate in such proportion that the ratio of hydroxyl groups to isocyanato groups is greater than 1, the coupled polyol being present in an amount sufficient to stabilize the res.ulting polymer/polyol.
In accordance with one aspect of this invention, the coupled polyols are prepared in situ in the base polyol by adding the rPquisite amount of the polyisocyanate to form the desired levei of coupled polyol. By this technique, it is possible to avoid any handling problems attendant with coupled polyols having higher than desired viscosities. Moreover, and significantly, in situ preparation of the coupled polyols should provide a lower viscosity for the resulting polymer/polyol in comparison to utilization of a separately prepared coupled polyol, later blended with the base polyol.

DESCRIPTION OF PREFERRED EMBODI~ENTS
The exact polyol, or blend or mixture, employed as the base polyol depends upon the end-use of the polyurethane product to be produced. For example, when foams are prepared, the molecular weight or the hydroxyl number is selected to result in flexible or semi-flexible foams. The polyols in this instance preferably possess a hydroxyl number of from about 50 to about lSO for semi-flexible foams and from about 25 to about 70 for flexible foams. As a further example, for elastomer applications~ it will generally be desirable to utilize relatively high molecular weight base polyols having relatively low hydroxyl numbers, e.g., 2~ to 50 or so. Such limits are not intended to be restrictive, but are merely illustrative of the large number of possible combinations for the polyol or polyols used.
The hydroxyl number is defined as the number of milligrams of potassium hydroxide required for the complete hydrolysis of the fully phthalated derivative prepared from l gram of polyol. The hydroxyl number can also be deFined by the equation:

OH = (5~.l x lOOO x f)/m.w.
where OH - hydroxyl number o~ the polyol f = functionality, that is, average number of hydroxyl groups per molecule of polyol m.w. - number average molecular weight of the polyol The most preferred base polyols employed in this invention include the poly(oxypropylene) polyols. Generally, the nominal functionality of l2895 :

such polyols will be in the range of about 3 to 4 or so. These polyols also include poly(oxypropylene-oxyethylene) polyols; however, desirably, the oxyethylene content should comprise less than 80 percent of the total and preferably less than 60 percent. The ethylene oxide, when used, can be incorporated in any fashion along the polymer chain. Stated another way~ the ethylene oxide can be incorporated either in internal blocks, as terminal blocks, or may be randomly distributed along the polymer chain. As is well known in the art, the polyols that are most preferred herein contain varying small amounts of unsaturation.
Unsaturation in itself does not affect in any adverse way the formation of the polymer/polyols in accordance with the present invention except in the case where the extent or type of unsaturation is so high as to result in a highly cross-linked polymer or gel.
While poly(oxypropylene) polyols are preferred, substantially 3ny of the polyols previously used in the art to make polymer/polyols can be used as the base po1yol in this invention.
Illustrative of the polyols useful in producing polymer/polyol compositions in accordance with this invention are the polyhydroxyalkanes, the polyoxyalkylene polyols, or the like. Among the polyols which can be employed are those selected from one or more of the following classes of compositions, alone or in admixture, known to those skilled in the polyurethane art:
(a) Alkylene oxide adducts of polyhydroxyalkanes;

l2895 ~ ~ '7~

- 17 _ (b) Alkylene oxide adducts of non-reducing sugars and sugar derivatives;
(c) Alkylene oxide adducts of phosphorus and polyphosphorus acids;
(d) Alkylene oxide adducts thereof of polyphenols;
- (e) The polyols from natural oils such as castor oil, and the like.
Illustrative alkylene oxide adducts of polyhydroxyalkanes include, among others, the alkylene oxide adducts of 7,3-dihydroxypropane, 1,3-dihydroxybutane, 1,4-dihydroxybutane, 1,4-, 1,5-and 1,6-dihydroxyhexane, 1,2-, 1,3-, 1,4-, 1,6-, and 1,8-dihydroxyoctane, l,10-dihydroxydecane, glycerol, 1,2,4-trihydroxybutane, 1,2,6-trihydroxyhexane, l,l,l-trimethylolethane, l,l,l-tr;methylolpropane, pentaerythritol, caprolactone, polycaprolactone, sylitol, arabitol, sorbitol, mannitol, and the like.
A further class of polyols which can be employed are the alkylene oxide adducts of the non-reducing sugars, wherein the alkylene oxides have from 2 to 4 carbon atoms. Among the non-reducing sugars and sugar derivat;ves contemplated are sucrose, alkyl glycosides such as methyl glucoside, ethyl g1ucoside, and the like, glycol glycosides such as ethylene glyco1 glucoside, propylene glycol glycoside, glycerol glucoside9 1,2,6-hexanetriol ~lucoside, and the like, as well as the alkylene oxide adducts of the alkyl glycosides as set forth in U.S. Patent No. 3,073,788.
A still further useful class oF polyols is the polyphenols, and preferably the alkylene oxide adducts thereof wherein the alkylene oxides have from 2 to 4 carbon atoms. Among the polyphenols .

which are contemplated are, for example, bisphenol A, bisphenol F, condensation prodwcts of phenol and formaldehyde, and novolac resins; condensation p~oducts of various phenolic compounds and acrolein;
the simplest member of this class being 1,1,3-tris(hydroxyphenyl) propanes9 condensation products of various phenolic compounds and glyoxal, glutaraldehyde, and other dialdehydes, the simplest members of this class being the 1~1,2,2-tetrakis (hydroxyphenol) ethanes, and the like.
The alkylene oxide adducts of phosphorus and polyphosphorus acids are another useful class of polyols. Ethylene oxide, lS2-epoxypropane, the epoxybutanes, 3-chloro-192-epoxypropane, and the like are preferred alkylene oxides. Phosphoric acid, phosphorus acid, the polyphosphoric acids such as tripolyphosphoric acid, the polymetaphosphoric acids9 and the like are desirable for use in this connection.
With regard to the coupled polyol constituent, it is preferred to use the poly (oxypropylene)polyols likewise preferred for the base polyol. However, any of the po1yols described dS useful for the base polyol may likewise be employed, depending upon the characteristics desired.
While coupled polyols made from diols are satisfactory for preparing polymer/polyols which are stable, such low functionality materials are undes;rable for use in preparing polyurethane foams and elastomers. These (and lower functionality) materials tend to adversely affect certain physical properties such as, for example, the static fatigue characteristics of such polyurethanes~ In accordance with this invention, the coupled polyols ~ ~ '7~

are therefore made utilizing polyols having a functionality 1n excess of 2Ø Preferably, the polyol employed has an average functionality in the range of about 2.5 to~4 or so, to provide urethane products with satisfactory physical properties, more preferably, a nominal triol is utilized.
It should be appreciated that, as with the base polyol, a blend or mixture of more than one polyol could be utilized, if desired, to form the coupled polyol.
Any of the known polyisocyanates utilized for forming polyurethanes may be employed in forming the coupled polyol. Toluene diisocyanate has been employed and allows preparation of the coupled polyol by a facile synthesis and may be preferred lS due to its commercial availability and price. Other polyisocyanates which have been satisfactorily utilized are: hexamethylene diisocyanate, methylene bis(4-cyclohexyl isocyanate) and MDI, diphenyl methane 4,4'-diisocyanate. Polymeric isocyanates having a functionality in excess of 2 such as, for example, polymeric MDI, should likewise be satisfactory.
The coupled po1yols may be made either in situ as previously described, or separately and then blended with the base polyol. When in situ preparation is utilized, the herein described advanta~es will be obtained. However, as is apparent, the polyol constituent will comprise those molecules of the base polyol coupled to the polyisocyanate employed. This will be quite satisfactory for many applications; however, there may be situations where it is desirable to utilize a polyol or polyols different from the base polyol for IL li ~7~3J~

the coupled polyol~ In those situations, the coupled polyol is prepared separately. For ex~mple9 separate preparation of the coupled polyol allows synthesis of higher molecular weight produ~ts than can be achieved with the in situ technique. Such higher molecular weight coupled polyols tend to be more effective in conferring stability to polymer/polyols. A penalty of increased viscosity will, however, be involved. The preparation technique utilized may then accordingly represent a balance between the effectiveness desired and the viscosity which can be tolerated.
In either technique, the synthesis of the coupled polyol may be carried out, for example, by feeding the polyisocyanate to the polyol which is being agitated and held at slightly elevated temperatures in the range of about 60 to 90C under an inert atmosphere, such as nitrogen. Optionally, be~ore or after completion of the feeding of the polyisocyanate, a catalyst such as dibutyltindilaurate can be added (e.g. - 20 p.p.m.), and the temperature held at the temperature of the agitated polyol until the product viscosity stabilizes. A period of about 2 to 4 hours wi1l generally be satisfactory. Other known catalysts for the reaction of an isocyanate with a polyol may be utilized, but it is preferred to use a catalyst that will not be adversely affected by materials such as a peroxide which might be present in the polyol utilized~
It will generally be desirable to utilize as great an excess of polyol in relation to the polyisocyanate as is possible, so as to minimize viscosity. In addition7 to avoid the presence of l2895 ~L~ 7~

free isocyanato groups, the polyol should be present in an amount sufficient to provide an excess of hydroxyl groups. Moreover, viscosity considerations are involved. Mole ratios of polyol to polyisocyanate of at least 2:1 are accordingly preferred. This will provide a ratio of hydroxyl to isocyanato groups ~with the functionalities of the polyol and isocyanate used) of about 2:1 to 3:1 in most instances. However, when formed separately, mole ratios as low as 3:2 or 4:3 may be employed to form relatively higher molecular weight coupled polyols. The limiting mole ratio will generally be determined by the viscosity level which can be tolerated.
Conceptually, the monomers used in lS preparing the polymer/polyols of this invention can comprise any ethylenically unsaturated monomer or monomers. A variety of monomers are disclosed in the prior patents relating to polymer/polyols previously referred to. The selection of the monomer or monomers used will depend on considerations such as the rela~ive cost of the monomers and the product characteristiCs required for the ;ntended app1ication.
The preferred monomer mixture used to make the polymer portion of the polymer/polyol compositions of this invention is a mixture of acrylonitrile and styrene. The relative weight proportions of acrylonitrile to styrene can range from about 80:20 to about 20:80. When it is desired to utilize higher polymer contents, useful ratios will tend towards higher acrylonitrile contents, e.g. - 80:20 to 50:50, more preferably, 80:20 to 70:30 for maximized polymer contents. For reduced scorch applications, it will generally be desirable to utilize ratios of 50:50 to 20:80, more preferably 40:60 or lower. However, when utilizing the present invention, stable polymer/polyols with relatively high polymer contents (e.g. - in excess of 30 weight percent or so) can be prepared, even with acrylcnitri1e to styrene ratios as low as 40:60 or so. To prepare virtually scorch-free, slab-stock foams of densities of 1.75 pounds per cubic foot or lower, it is preferred to utilize a ratio o~ about 30:70 or lower.
It may be desirable in some applications to utilize, with acrylonitrile, a comonomer other than styrene. Representative examples of suitable comonomers include methyl methacrylate, vinyl lS chloride and vinylidene chloride.
The polymer content of the polym~r~polyol can vary within wide limits, depending upon the requirements of the anticipated end use application.
It will usually be desirable to form the polymer/polyols with as high a polymer content as will provide the desired viscosity and stability properties. In general, this will vary from about 10 to about 50 percent, based upon the weight of the polymer/polyol. Lower polymer contents may, of course, be utilized; however, there is typically no incentive to use monomer amounts which will result in polymer contents lower than about 10 percent by weight because of the lower conversions and the economic penalty due to the increased throughput involved. On the other hand, it will generally be undesirable to utilize polymer contents in excess of about 40 percent by weight or so. While useful polymer/polyols with higher polymer contents 1~'7~

certainly can be made, such polymer/polyols may possess viscosity and stability characteristics which are commercially undesirable.
The polyol content of the polymer/polyol varies from about ~0 to about 90 percent, based upon the weight of the polymer/polyol. The relative amount of the coupled polyol utilized will depend upon the parameters involved, viz. - the relative amount of polymer, the particular monomer or monomers used, the molecular weight of the base polyol and the polymer/polyol stability characteristics required. Functionally, the coupled polyol should be present in an amount sufficient to provide the desired polymer/polyol stability characteristics. In general, the amount required to accomplish such characteristics will increase with increasing polymer contents and decreasing acrylonitrile:styrene monomer ratios and base polyol molecular weight~ It should be suitable to satisfy most situations by including the coupled polyol in an amount in the range of from about 5 to about SO
percent, based upon ~he total weight o~ the base polyol and a 2:1 mole ratio of polyol to polyisocyanate. If a polyol to polyisocyanate ratio in excess of 2:1 is employed, the weight of such reaction product should be increased accordingly.
For example, if a ratio of 4:1 is used, it would be expected that, on the average, 50% of the polyol molecules would be unreacted and the other ~0% would appear as 2:1 coupled polyols. On the other hand, if a ratio of less than 2:1 is utilized, the molecular weight of the coupled polyol will be higher; and the amount of such reaction product required for effective stabilization should be ~'7~
.
- 2~ -somewhat redllced. The description herein is predicated on the functionality of the polyisocyanate being 2, viz. - 2 polyol molecules being couple~ to one diisocyanate molecule. If a higher functionality polyisocyanate is used (e.g. -a polymeric isocyanate), the average molecular weight of the resulting coupled polyol will be somewhat higher requiring an adjustment in the amount of coupled polyol needed.
The polymer/polyols of this invention are produced by polymerizing the monomer system used in the presence of a free radical catalyst in the polyol mixture of the base and coupled polyols. The polymerization can also be carried out with an inert organic solvent present that does not dissolve the lS polymer. Illustrative of such solvents are xylol, toluene, benzene, acetonitrile, ethyl acetate, hexane, heptane, dicyclohexane, dioxane, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, and the like, including those known in the art as being suitable solvents for the polymerization o~ vinyl monomers. The only requirement in the selection of the solvent and the polyol is that they do not interfere with the polymerization reaction. When an inert organic solvent is used, it is generally removed from the reaction mixture by conventional means before the polymer/polyol is used to produce polyurethane foams.
The polymer/polyols of the present invention are preferably produced utilizing the process set forth in the previously identified Priest et al. patent. In accordance with that process, a low monomer-to-polyol ratio is maintained throughout the reaction mixture during the process.

This is achieved by employing process conditions that provide rapid conversion of monomer to polymer.
In practice~ a low monomer-to-polyol ratio is maintained, in the case of semi-batch and continuous operation, by control of the temperature and mixing conditions and, in the case of semi-batch operation, also by slowly adding the monomers to the polyol.
The temperature range is not critical and may vary from about 100C to about 150C, or perhaps greater, the preferred range being from 115C to 135C. As has been noted herein, the catalyst and temperature should be selected so that the catalyst has a reasonable rate of decomposition with respect to the hold-up time in the reactor for a continuous flow reactor or the feed time for a semi-batch reactor.
Catalysts useful in producing the polymer/polyol compositions of this invention are the free radical type of vinyl polymerization catalysts such as the peroxides, percarbonates and the azo compounds or any other suitable catalyst specified in the above-mentioned patents. Azo catalysts such as azobis (isobutyronitrile) are the preferred catalysts.
The catalyst concentration is not critical in most applications and can be varied within wide limits. As a representative range, the concentration can vary from about 0.1 to about 5.0 weight percent, based upon the total feed to the reactor. Up to a certain point, increases in the catalyst concentration result in increased monomer conversion but further increases do not substantially increase conversion. Conversions of monomers to polymers which can be typically achieved are on the order of 85 to 95% of the monomer charged. On the other hand, increasing catalyst concentration increasingly improves product stability. The catalyst concentration selected will usually be an optimum value considering all factors, including cos~s.
The mixing conditions employed are those attained using a back mixed reactor (e.g. - a stirred flask or stirred autoclave). Reactors of this type keep the reaction mixture relatively homogeneous and so prevent localized high monomer-to-polyol ratios.
The utili~ation of the Priest et al.
process is preferred since this allows the preparation of polymer/polyols with a wide range of monomer compositions, polymer contents, and base polyol that could not be otherwise prepared with the necessary requisite stability. However, whether the utilization of the Priest et al. process is essential depends upon whether the process parameters are such that a satisfactory polymer/polyol can be prepared without using this process.
In addition, it shou1d be appreciated that other of the previously mentioned prior techniques can be utilized in forming the polymer/polyols so long as the required product characteristics are not, of course, adversely affected to any significant extent. For example, there may be particular situaticns where it would be desirable to incorporate added unsaturation to the base polyol, such as by the addition of a minor amount of a glycidyl ether, such as allyl glycidyl ether, or by utilizing a more reactive double bond.

l2895 ~7~

The polymer/polyols produced in accordance with this invention are characterized by highly desirable stability characteristics. The filtration and centrifugibility performance is indicative of such stability. The filtration characteristics are determined by passing a sample of the polymer/polyol by gravity, through~ successively, two wire screens. The most stable polymer/polyols will pass completely through such screens (i.e.~ over 99 weight percent), and this type of performance is preferred. It may be suitable, however, in some applications to provide filtration performance down to 50% or even somewhat less.
Stability is also confirmed by the amount of material (cake) which is thrown down from samples placed in laboratory centrifuges. This is, in effect, an accelerated settling test, primarily, indicative of storage stability. In general, the lower the amount of centrifugible solids obtained, t`he more stable is the polymer/polyol.
~0 Fro~ the functional standpoint, suitable polymer/polyols must be capable of: (1) being made~
(2) stored, ~3) shipped and (4) used without undue loss of polymer content or damage or fouling of the equipment in which it is made and handled. If a polymer/polycl meets these functional criteria, it is considered satisfactorily stable.
The present invention also provides a method for producing polyurethane products by reacting: (a) a polymer/polyol composition of this invention, (b) an organic polyisocyanate, and (c) a catalyst for the reaction of (a) and (b) to produce the polyurethane product, and, when a foam is being prepared, a blowing agent and a foam stabilizer.

The reaction and foaming operations can be performed in any suitable manner, preferably by the one-shot technique.
The polymer/polyol may, if desired, be blended with conventional polyols or the like to reduce the polymer content to the level required for the particular end use application. Blends in which the resulting polymer content is as low as 4 percent of the total weight of the blend or even less are useful.
The organic polyisocyanates that are useful in producing polyurethane products in accordance with this invention are organic compounds that contain at least two isocyanate groups. Such compounds are well kno~n in the art. Suitable organic polyisocyanates include the hydrocarbon diisocyanates, (e.g., the alkylene diisocyanates and the arylene diisocyanates) as well as known triisocyanates. As examples of suitable polyisocyanates, one can mention methylene bis(4-cyclohexyl isocyanate), MDI, polymeric MDI, 1,2-diisocyanatoethane, 1,3-diisocyanatopropane, 1~2-diisocyanatopropane9 1,4-diisocyanatobutane, 1,5-diisocyanatopentane, 1~6-diisocyanatohexane~
bis(3-isocyanatopropyl)ether, bis(3-isocyanatapropyl) ~5 sulfide, 1,7 diisocyanatoheptane, l,S-diisocyanato-2,2-dimethylpentane, 1,6-diisocyanato-3-methoxyhexane, 19 8-diisocyanatooctane~
1,5-diisocyanato-2,2,4-trimethylpentane~
l,9-diisocyanatononane, l,10-diisocyanatopropyl) ether of 1,4-butylene glycol, l,ll-diisocyanatounde-cane, 1,12-diisocyanatododecane bis(isocyanatohexyl) sulfide, 1,4-diisocyanatobenzene, 2,4-diisocyanato-toluene, 2,6-diisocyanato tolylene, 1,3-diisocyanato-~ 9 7 ~ I~J, L'~ ~
- 29 ~

o-xylene, l,3-diisocyanato-m-xylene, 1,3-diisocyanato-p-xylene, 2,4-diisocyanato-1-chlorobenzene~ 2,4-diisocyanato-1-nitrobenzene, and 2,5-diisocyanato-1-nitrobenzene and mixtures thereof.
Any known catalysts useful in producing polyurethanes may be employed. Representative catalysts include: (a) tertiary amines such as bis(dimethylaminoethyl)ether, trimethylamine, triethylamine, N-methylmorpholine, N-ethylmorpholine~ N,N~dimethylbenzylamine, N,N-dimethylethanolamine, N,N,N',N'-tetramethyl-1,3-butanediamine, triethanolamine9 1,4~diazabicyclo~2.2.2~octane, pyridine oxide and the like; (b) tertiary phosphines such as trialkylphosphines, dialkylbenzylphosphines, and the like; (c) strong bases such as alkali and alkaline earth metal hydroxides, a1koxides, and phenoxides;
(d) aci-dic metal salts of strong acids such as ferric chloride, stannic chloride, stannous chloride, antimony trichloride, bismuth nitrate and chloride, and the like; (e) chelates of various metals such as thosé which can be obtained from acetylacetone, benzoylacetone, trifluoroacetyl-acetone, ethyl acetoacetate, salicylaldehyde, cyclopentanone-2-carboxylate, acetyl-acetoneimine, 2S bis-acetylacetone-alkylene-diimines, salicylaldehydeimine, and the like, with the various metals such as Be, Mg, Zn, Cd, Pb, Ti, Zr, Sn, As, Bi, Cr, Mo, Mn, Fe, Co, Ni, or such ions as MoO2+~, U02~+, and the like; (f) alcoholates and phenolates of various metals such as Ti(OR)4, Sn~OR)4, Sn(OR)2, Al(OR)3, and the like, wherein R is alkyl or aryl, and the reaction products of alcoholates with carboxylic acids, 7~L¢~ -betadiketones, and 2-(N,N-dia1kylamino)alkanols, such as the well known chelates of titanium obtained by said or equivalent procedures; (g) salts of organic acids with a variety of metals such as alkali metals~ alkaline earth metals, Al, Sn9 Pb, Mn, Co9 Ni, and Cu, including, for example, sodium acetate, potassium laurate, calcium hexanoate9 stannous acetate9 stannous octoate, stannous oleate9 lead octoate, metallic driers such as manganese and cobalt naphthenate, and the like; (h) organometallic derivatives of tetravalent tin, trivalent and pentavalent As, Sb, and Bi3 and metal carbonyls of iron and cobalt.
~mong the organotin compounds that deserve particular mention are dialkyltin salts of carboxylic acids, e.g. dibutyltin diacetate, dibutyltin dilaurate, dibutyltin rnaleate, dilauryltin diacetate, dioctyltin diacetate, dibutyltin-bis(4-methylaminobenzoate), dibutyltin-bis(6-methylaminocaproate), and the like. Similarly9 there may be used a trialkyltin hydroxide, dialkyltin oxide9 dialkyltin dialkoxide, or dialkyltin dichloride. Examples of these compounds include trimethyltin hydroxide, tributyltin hydroxide, trioctyltin hydroxide, dibutyltin oxide, dioctyltin oxide, dilauryltin oxide, dibutyltin-bis (isopropoxide)~ dibutyltin-bis(2-dimethylamino-pentylate), dibutyltin dichlorideg dioctyltin dichloride, and the like.
The tertiary amines may be used as primary catalysts for accelerating the reactive hydrogen/
isocyanate reaction or as secondary catalysts in combination with one or more of the above noted metal catalyst. Metal catalysts, or combinations of 12~95 . gl~ '7~ r metal catalysts, may also be employed as the accelerating agents, without the use of amines. The catalysts are employed in small amounts, for example, from about 0.001 percent to about 5 percent, based on the weight of the reaction mixture.
When the product being formed is a polyurethane foam, this may be accomplished by employing a small amount of a polyurethane blowing agent, such as water, in the reaction mixture (for example, from about 0.5 to about 5 weight percent of water, based upon total weight of the polymer/po1yol composition), or through the use of blowing agents which are vaporized by the exotherm of the reaction, or by a combination of the two methods.
Illustrative polyurethane blowing agents include halogenated hydrocarbons such as trichloromonofluoro-methane, dichlorodifluoromethane, dichloromonofluoro-methane, dichloromethane, trichloromethane, 1,1 dichloro-l-fluoroethane, 1?1,2-trichloro-1,2,2-trifluoromethane, hexafluorocyclobutane, octafluorocyclobutane, and the like. Another class of blowing agents include thermally unstable compounds which liberate gases upon heating, such as N,N'-dimethyl-N,N'-dinitrosoterephtha1amide, and the like. The generally preferred method of foaming for producing flexible foams is the use of water or a combination of water plus a fluorocarbon blowing agent such as trichloromonofluoromethane. The quantity o~ blowing agent employed will vary with factors such as the density desired in the foamed product.
The anti-scorch properties of the foams produced using polymer/polyol compositions are most evident when at least some of the blowing agent is water and the water ls used in an amount that results in a foam having a density less than 1.75 pounds per cubic foot. Generally, the use of water in an amount of at least 3.0 percent by weight based on the ~otal ~eight of the polymer/polyol composition results in a foam having a density of less than 1.75 pounds per cubic foot.
It is also wlthin the scope of the invention to employ small amounts, e.g., about 0.001 percent to 5.0 percent by weight, based on the total reaction mix~ture, of a foam stabilizer ~uch as a "hydrolyzable" polysiloxane-polyoxyalkylene block copolymer such as the block copolymers described in the U.S. Patents 2,834,748 and 2,917,480. Another useful class of foam stabilizers are the "non-hydroly~able~ polysilo~ane-polyoxyalkylene block copolymers such as the block sopolymers described in U.S. Patent 3,505,377; U.S. Patent 3,686,254 and the British Patent Specification 1,220,471. The latter class of copolymers differs from the above mentioned polysiloxane-polyoxyalkylene block copolymers in that the polysiloxane moiety is bonded to the polyoxyalkylene moiety through direct carbon-to-silicon bonds, rather than through carbon-to-oxygen-to-silicon bonds. These various polysi1oxane-polyoxyalkylene block copolymers preferably contain from 5 to 50 weight percent of polysiloxane polymer with the remainder being polyoxyalkylene polymer.
The polyurethanes so produced may be utilized in foam and elastomer applications where any conventional type of polyurethane is or can be utilized.

!~
/, ^ , ~ 7~

The following Examples are illustrative of, but not in limitation of, the present invention.
These Examples describe the preparation of coupled polyols, the use of coupled polyols in the preparation of polymer polyols and the preparation of polyurethane foams from such polymer/polyols.

DEFINITIONS
As used in the Examples appearing below, the following designations, symbols, terms and abbreviations have the indicated meanings:
"Theoretical molecular weight" of a polyol denotes a molecular weight calculated using the equation previously set forth based on the functionality of the starter used to produce the polyol and the experimentally determined hydroxyl number of the polyol.
"Molecular weights" of polyols are number average molecular weights.
"rpm" denotes revolutions per minute.
"g" denotes grams.
"mg" denotes milligrams.
"TDI" denotes toluene diisocyanate.
"HMDI" denotes hexamethylene diisocyanate.
"MDI" denotes diphenylmethane 4,4'-diisocyanate.
"Desmodur W" denotes methylene bis(4-cyclohexyl isocyanate).
"VAZO-64P" denotes 2,2'-azobis(isobutyro-nitrile).
"TMSN" denotes tetramethylsuccinonitrile.
"pcf" denotes pounds per cubic feet.
"Sol" denotes solution.
"S" denotes solid.

l2895 "%" denotes percent by weight.
"wt" denotes weight.
"Ratio" denotes weight ratio.
"GPH" denotes gallons per hour.
"conc." denotes concentration.
"cks" denotes centistokes.
"cps" denotes centipoise.
"hr." denotes hour.
"sec." denotes seconds.
"calc." denotes calculated.
"ppm'l denotes parts per million.
"T-12" denotes dibutyltindilaurate.
"Polyol I" is a polypropylene oxide triol (the designation of this and subsequent polyols as a "triol" or "diol" represents the nominal functionality based solely on the starter used; the actual functionality will be somewhat less) having about lOX external ethylene oxide content, a hydroxyl number of about 48 and a number average molecular weight of about 3300.
"Polyol II" is a polypropylene oxide diol having about 15% external ethylene oxide content, a hydroxyl number of about 38 and a number average molecular weight of about 2800.
"Polyol III" is a polypropylene oxide triol having about 14% interna1 ethylene oxide content, a hydroxyl number of about 47 and a number average molecular weight of about 3300.
"Polyol IV" is a polyol produced from sorbitol and glycerine having an external ethylene oxide content of about 15%, a hydroxyl number of about 28 and a number average molecular weight of about 7100.

~:~'7~

"Polyol V" is a polypropylene oxide triol having an external ethylene oxide content of about l5%, a hydroxyl number of about 27 and a number average molecular weight of about 4400.
"Polyol VI" is a polypropylene oxide triol .having an internal ethylene oxide content of about l4%, a hydroxyl number of about 24 and a number average molecular weight of about 5000.
"Polyol VII" is a polypropylene oxide triol having an internal ethylene oxide content of about 8%, a hydroxyl number of about 56 and a number average molecular weight of about 2800.
"Polyol VIII" is a polypropylene oxide triol having an internal ethylene oxid~ content of about l6.5X, a hydroxyl number of abou~ 35 and a number average molecular weight of about 4000.
"Polyol IX" is a polypropylene oxide triol having an external ethylene oxide content of about l7%, a hydroxyl number of about 39 and a number average molecular weight of about 4200.
"Polyol X" is a polypropylene oxide triol having an internal ethylene oxide content of about lO%, a hydroxyl number of about 50 and a number average molecular weight of about 3100.
"Polyol XI" is a polypropylene oxide triol having an e~ternal ethylene oxide content of about l5%, a hydroxyl number of about 35 and a number average molecular weight of about 4000.

POLYMER/POLYOL PROPERTIES

Filtration Hindrance (Filterability) This is determined by diluting one part by weight sample (e.g. - 470 grams) of polymer/polyol l2895 with two parts by weight anhydrous isopropanol (e.g.
- 940 grams) to remove any viscosity-imposed limitations and using a fixed quantity of material in relation to a fixed cross-sectional area of screen ~e.g. - 1.8 sq. inO) such that about 200 grams of product are passed by gravity through 150 or 700-mesh screen per one square inch of screen.
The difference between the final and initial screen weights corresponds to the amount of polymer that did not pass through the screens. The 700-mesh screen is made with a Dutch twill weave. The actual screen used had a nominal opening of 30 microns and is described in Bullet;n 462h7-R of the Ronningen~Petter Company of Kalamazoo, Michigan.
The 150-mesh screen has a square mesh with average mesh opening of 105 microns, and it is a "Standard Tyler" 150 square mesh screen. The amount of solids that did not pass through the screens is reported as parts of solids per million parts of the original undiluted sample. The amount of sample which passes through the screens is reported in percent, a percentage of 1~0% being preferred. Trace solids will generally always be present, but a value of lOOX indicates that over 99 weight percent passes through the screen.

Centrifu~ible Solids After stripping unreacted monomer, the polymer/polyol composition is centrifuged for about 24 hours at about 3000 revolutions per minute and 1470 radial centrifugal "9" force. The centrifuge tube is then inverted and allowed to drain for 4 hours. The non-flowing cake remaining at the bottom of the tube is reported as weight percent of the initial weight of the composition tested~ To provide a commercially satisfactory stable polymer/polyol, the solid should be less than about lO%, preferably less than about 5%.
PREPARATION OF COUPLED POLYOLS
Unless otherwise indicated9 the coupled polyols were prepared generally as follows. The polyol and catalyst were charged to a reaction flask equipped with a mechanical agitator and maintained under a nitrogen atmosphere. The polyol was continuously agitated and heated to about 80C and then the diisocyanate was slowly added to the polyol. The reactants were maintained at a temperature of from about 70 to about 80C for two to four hours after the addition of the diisocyanate.
Thereafter, the product was cooled and stored without further processing.
PREPARATION OF POLYMER/POLYOLS
.. . . . . _ Unless otherwise indicated, the polymer/polyols were prepared in a single-stage, continuous, back-mixed reactor having four internal equally spaced vertical baffles and equipped with a mechanical agitator. Two feed streams, one comprising a premix of the selected monomers and catalyst and the other comprising the polyol feed (the polyol feed consisting of base polyol and the coupled polyol~ were added simultaneously through an in-line mixer to the reactor and agitated therein.
The reactor was heated initially to a temperature of about 135C and then the temperature was adjusted to that shown in the Examples. The feeds were continued for 90 minutes line-out before the product was collected. Product collected from the reactor was stripped at 130C with a nitrogen sparge and then cooled to 35C.

l2895 FOAM PREPARATION
Molded, water-blown~ flexible polyurethane foams having an Index of 103 wer~ prepared using polymer/polyols, 3.5 parts water and a p31yi socyanate reactant comprising a mixture of tolylene diisocyanate and polymeric MDI at a weight ratio of, respectively, about 80 to 20.
Standard foam formulations comprising polymer/polyol, tin catalyst, surfactant, water and amine catalyst were converted to polyurethane foams using the following procedure. The polymer/polyol, tin catalyst and surfactant were charged to a 1/2 gallon paper container and mixed at 4000 rpm for 30 seconds with a 2.5 inch 6-blade turbine stirrer (placed one inch above the bottom of the container).
Water and amine catalyst were added and mixing continued for an additional 55 seconds. Stirring was stopped for 25 seconds to de-gas. The polyisocyanate reactant was added and mixing continued for 5 seconds. The foaming mixture was poured quickly into a 15 inch x 15 inch x 4-1/2 inch aluminum mold (mold temperature of about 120F) having four 1/16 inch vent holes drilled 5 inches diagonally from each corner in the lid. The mold was clamped and the foam was allowed to rise and gel. The foam was demolded after 8 minutes~

These Examples illustrate the preparation of coupled polyols utilizing Polyol I (Examples 1 and 2), and mixtures of Polyols I and II (Examples 3 and 4). Tolylene diisocyanate was the polyisocyanate used in each Example.

_ 39 _ The specific process parameters used and the properties of the coupled polyols are set forth in Table I:

.
~
Polyol I, gm 17561 17420 8274 6506 Polyol II, gm -- -- 8274 6506 Temperature, C 75-80 75-80 75-80 75-80 Tolylene diisocyanate, 10. gm 439 580 452 473 Time to feed TDI, hours 0.5 0.75 1 0.25 Mole ratio polyol: TDI 2.10:1 3.16:2 2.10:1 3.16:2 T-12 catalyst, ppm 20 20 20 20 Temperature, C 75-80 75-80 75-80 75-80 lS Time, hours 2 2 3 4.5 Viscosity, cks at 25C
after 1 hour 4555 16653 7518 26874 after 2 hours 4542 16325 7589 28943 after 4 hours -- -- -- 28265 Final analysis Hydroxyl No., mg KOH/gm 32.3 26.5 24.7 20.3 theoretical 31.4 25.9 24.9 19.1 Acid No., mg KOH/gm 0.02 0.06 0.04 0.02 Viscosity, cks at 25C 4603 16325 7539 27200 at 130F 942 3034 1516 4770 at 210f 217 638 347 1004 Primary hydroxyl, X 48.3 47.2 52.4 45~2 Functionality, theoretical 3.6 4.3 2.6 2.9 Molecular weight 6253 9103 5905 8014 These Examples illustrate the preparation of coupled polyols using polyisocyanates other than tolylene diisocyanate. The specific process parameters used as well as the properties of the resulting coupled polyols are set forth in Table II:

TABLE II
_ ~ 7 Example No. 5 Polyol: Type VII VII VII
gm 3696 3641 3648 Isocyanate: Type HMDI Desmodur W MDI
Mole ratio, polyol: isocyanate 2.1:1 2~1:1 2.1:1 Temperature, C 70 75 75 T-12 catalyst, ppm 20 20 20 Temperature, C 80 80 80 Time, hours 4 7 3 Viscosity, cks at 25C
After 1 hour 3150 4590 5785 3 hours 3485 -- 5754 4 hours 3485 4980 --7 hours -_ 5090 __ Final analyses Hydroxyl No., mg KOH/gm 37.5 37.0 37.9 Theoretical 38.2 37.7 37.7 Acid No., mg KOH/gm 0.02 0.01 0.06 Color, Pt-Co 20 20 20 Yiscosity, cks At 25C 3468 5098 5724 Functionality, theoreticall 3 7 3.7 3.7 Molecular Weight 5535 5610 5477 1. Assumes a functionality of 2.9 for Polyol YII and an isocyanate purity of 100%.

These Examples illustrate the preparation of polymer/polyols utilizing the present invention and, for comparative purposes, polymer/polyols made with a blend of Polyol III and particular high molecular weight polyols. No comparative example is set forth using Polyol III by itself since, under the conditions set forth herein, a stable polymer/
polyol could not be prepared.
Examples 8-15 illustrate the preparation of polymer/polyols using a polyol mixture of Polyol III

~L~'7~

. .

as the base polyol and coupled polyols from prior Examples at a weight ratio, respectively, of 85 to 15. Examples 16-18 are illustrative of polymer/polyols made from blends of Polyol III and the indicated high molecular weight polyols (made by conventional techniques) in the same weight ratio used for Examples 8-15.
The specific process parameters as well as the properties of the polymer/polyols are set forth in Table III:

01 -- ~ ~ ~ ~ ~ -- -- ~ ~ 0 'O ~ . 0 . r~ ~r~ O r~ o --_ O c~ -- 0 ~` 0 ~ 1'1 _ ~
1~ 1 (~ o ~ 0 a' ~ 0 1~ 0 ~ 0 _ ~ 0 0 ~ O ~7 I ~~ ~ ~ ~ ~ ~ _ _ o 0 c~
O C~
r u7 o u- 1~ (~1 _ o a~ o--o ~
r~ ~ ~ ~ o 0 C~ 0 o ~ _ cr~
-- O ~ C~J
r ~ O ~ J O ~ O ~S O 1~ 0 C~
O C~J _ I _ _ . ~ 0 . O ~r ~s ~ ~7 ~ _ . . ~r . ~s O O ~D $--_ O C~l n 'n 'n 0 ~ ~ - o ~:r o ~ c C~J o ~ - o o s oJ ~D oo ~ O ~_ --I ~ ~ ~ C`' O C`~ C~J ~ ~ 0 0 o~ 0 o ~ ~ 00 3700 O 3~ O~ O~r 1~1O ~ Cl~--~ ~Or~ ocl~
~I ~ # ~ --O 3~ 3~ 0 ~ ~ ~ ~
_ O C~
r ~ o ~ ~ ~r In 0 0 ~.~ r~ 1~ ~ r~ 3~ ~ O ~ O r~
O O O 1~ _ r~ ~ ~ _ _ O ~; 3~ ~ r ~ O
. O ~
r~ o~ ~ o--C --. ~ ~ ~ c o~ r~) r~ In ~ _ o m o lo n O ~ ~ . _ U:l . . . _ ~ In . ~n o o. _ C`~ _ --I ~ #~ --o~rrJ0 O~
~ o~ In o ~ O~ o ~ ~ ~ 10 ~ ~0 ~n o ~ o ~ 8 ~
X Cl~ ~ ID _ ~ . ~ ~ _ _ O a~ 3~ 0 ~ ~ C~
_ O C~l ~ ~ O 1n . _ 1~. ~ _ ~ r- r- G~ r- ~ r~ ~ O, ~ ~ O ~ O = c~
X ~ r~ . ~ O:~J ----O 0 ~ J O 1~7 _ ~ O
~ O ~ ~r ~
Q
vl E ~ CJ
Q
o C~ X
'n c cJ ~ ~L Q ~ v 2 ~CJ 3 c ~ c c C ~ ~ cJ
è ~ O O U O U ~~
U C ~ cn 3 ZC ''I L Vl ~ ~-- _ c~u 3 c; ~ 'J ~ ~
I U CJ ~ _ V-Cl C;'L -- 3 -- ' ~ ~ O C C
C -- ~ ClC CJ _ ~ IJ -- ~ -- CJ O C~ o C
C 3C e ~ O L lle ^ L ~ C C 3 ~ L ~ 1 o o E u IU-- Z û CJ O -- ~ O L ~ O ~
L _ ~L ~ L ~ y ~ L e~ el CJ . ~ -- _ E
z x O--O~ O O x )--~ + cu cJ + ~ O E O O -- ~ O
CJ. ~ CJ CJ ~ v~ ~ O ~r L L ~ O ~ CJ
_ _ ~ c :~ o ~ ~ cJ -- cE cJ _ o v L CJ l.J ~
el_ 3~ ~ C ~ ~ C 'v~ I L o J
I.JcO, O Cl O O O CJ LOJ ~' L ~ _ The centrifugibility of the polymer/polyols was determined in accordance with ;the procedure set forth above. Similarly, the filterability of the polymer/polyols was determined as set forth above using 200 gms of unstripped sample diluted with 400 grams of anhydrous isopropanol and screens each having an area of about 1.8 square inches.
As can be seen from the aboYe results, the polymer/polyols made in accordance with the present invention tend to have lower centrifugible solids levels than the polymer/polyols utilizing polyols made by conventional techniques. Moreover, such conventicnal techn;ques would be expected to result in diminution of the functionality of the lS polymer/polyols (in eontrast to the functionality of the polymer/polyols made pursuant to the present invention) which could well adversely affect certain physical properties, such as static fatigue9 in derived polyurethane foams.

This Example illustrates a relatively large scale production of coupled polyol formed by the reaction of 2 moles of Polyol XI with 1 mole of tolylene diisocyanate.
A 100-gallon, glass-lined, steel reactor, equipped with a three-blade, retreat-curve, 24-inch diameter impeller was used. This was operated at 190 rpm to agitate the feed, 828 pounds of Polyol XI.
The polyol was heated to 70C-80C under a nitrogen atmosphere. Tolylene diisocyanate was next added to the reactor through a pump rated at 9.8 GPH at a rate such that 22.0 pounds of the isocyanate was charged within 45 minutes. Then 7.7 gm of T-12 catalyst, equivalent to 20 ppm, were added, and the reaction temperature increased from 73C to 79C.
The reaction temperature was maintained at a temperature of about 77-78C for 2.5 hours. The reaction product was then cooled and stored.
The coupled polyol thus prepared had a hydroxyl number of 32.8 mg KOH/gm, a viscosity at 25C of 4840 cks and a functionality of 3.9.

EXAMPLES 20~28 These Examples illustrate the preparation of coupled polyols fo110wing the procedure set forth above using tolylene diisocyanate and Polyols VIIIg IX and XI at various mole ratios of polyol to isocyanate. The reaction parameters and coupled polyol properties are set forth in Table IV:

- 45 - _ ,~
o a: X ~ o ~ ~ o .. o oa ~ = -- ~--O
-- ~O ~ -- O 3 o C~'~-- `Cl~ 3 0 C`l ~ U~
1--x ~ o o~o o ~ o r~-- r~
c`l -- ~`I r O 1 ~ ~ 3 3 1~ 0 ~O O ~
v 3 ..:1- tr, Ll~ a~ CD O
~J O 3 0 ~ O O
~, _ ~ ~ ~ .:t O
O V

Lr~ X ) O OCO o ~ O~ 3 o 1~ ~o ~ Lt~ o o a O ~ 3 --o a~
X ~ ~' ~ ~ a~ "'I ''" I~

~ .
= ~ o ~ o ~ ~a'\ 3 c~J -- ~-- I1~ --co ~ oo cr~ _ o 3 ~ O ~ . O
~ X
J --0 _ co ~ ~ o o a~ u~ - O ~D ~ ~ O a~ 0 -- - ~ r~ I~ ~ O co c~l co O CO
U~
Ul _ 5 ~ E
c~ _ - ~ ~ C`~ 3 co C~l f~ Ln 'a o ~o o ~ _~ ~-- O ~
E

-- O -- Co o -- a~ o o a~ o - o ~ o a~ co ~
j~ 1~ C C`~ C0 C0 3 . ~ 0 V
:t' ~ ~ C~ O ~ ~

U
~11 U~
~ O --'J E o v V o ~ O
-- C`~ E ~ a.l r ~ ~ ~) c 3 O E - cn ~ ~ v v Q O U~ O ^ co ^O ~ --o ~ ~
Q vo o ~ 3 ~
E Q~ C' a.~ V ~ ^ al ~ --X >` -- ~1 o -- ~ V . C ~ o ~J V V V o U~ X O Ul Z ~
~E O ~ 5 C a) o ~ o v ~ ~
-- E ~ ~ cn V u~ C ~ C
O cn -- -- E E~ -- E E ~ ~ ¢
O I a~ C~ ~-- O ~ ~-- C
CL 1-- ,_ ~ 1_ 'F l_ ~ ¢

~7~
. .

Since all of the polyol to isocyanate ratios used are in excess of 2:1, unmodified polyol molecules will be present as well as coupled polyol molecules. As can be seen, as such ratios increase, the relative amount of unmodified polyol molecules likewise increase; and the viscosity of the mixture decreases.

These Examples illustrate the comparison of polymer/polyols made only using Polyol VIII with polymer/polyols made in accordance with the present invention at acrylonitrile to styrene ratios ranging from 50:50 to 30:70.
The reaction parameters and resulting polymer/polyol properties are set forth in Table V:

H ~ ('f) ~1t--a~ 0 Lf~ ~) 0 1--C\J 0 U~ L ~ ~ ~ H 0 CO ~ O ~ O It~
O H ~O ~ (`'1 C~i \D ~) ~D 0 ~, ~I N ~ l i~ 0 N O
H 0 r~ 0 ~ 0~ H O H U~ ~:t IJ~ U~ 0 . ~i O
~ ~ ~C 0 ~ ~ C\i O ri ~ C~i O C~J O 0 0 ~ 0~
Ll'~ H . t~ O ~-- ' O O ~t ~D ~D 1~ Yi ~ ~ ~ C~ ~ O 0 0 0 0 cl`\ H CU O ~D H (Y') O i I I H H - (rl ~ O O
- H 0~ O IJ~ O ~ l O r-l ~ 11~ ~ \.D N ~I H
C~l ~ \D~ ~ r~l o c~ 0 0 a~
~i CU ~i C~
H ~ ~) ~- :J CO H 11~ ~ O C--C~l O 0 ~) 11~ H ~t ~O 0 0 0 ~ O ~1 a:~ H C\~l O ~ N ~ CO Lr~ 0 0 H CU \~ O 0 0 (rl ~i ~O H X C~l O C`J O 0 0 0 0 il~. ~t 0~ N
C~i H OO O Ll~ ~O O ~:t O O
1~ H O ~ O O O IA C'J I I ~ I I I I I I I I I I C~ O O

H O O o~ O O ~ i ~t ~) H 0 (rl o~ O 3 1S~ o 0 ~:) H O C~J O O u~0 C~ ~ o ~1 H ~ l lA r-l H C\i ~1 O O ~ ~ 0 u~ ~ ,i 0 ,1 (rl Q ~ i ~i ~1 0 0 C'~ 0 ~
r~
H 0 ~ C~i~1 ~ri 0~ u~D N ~ ~D O \D ~ O C~ ~ ~ o 0 ~1 H 11~~ ~ H o O ~ ~O O a~ H r~
0 X r~ (~ o \0 ~ c~i ~1 ~i o co a~ 0 ~ c~
~ C~i C~i H ('-i 0 U~ 0 ~ 0 ~ O rl Cl~ ~ ~ O ~0 O C0 Hc0 ~ 0 0 0 t-- ~ 0 r~
CU
H ~ 0 U~ 0~ Hi ~O H U~ O ~ 1 0 L~ ~ ~ O ~i O t--~)H I I II H N 0 U~ ~ N C~.l ~i CS~ 0~ O O
i 0 ~ ~ o ~NO ~ N ~ r-i ~i 0 0 O~ ~ ~ N N 0 ~ N
H ~ Hi r~ ~0 ~0 Ct ) ~ ~0 H O C~l O ~ ~D O O O
C~l H I I I I r-l N C-- ~ ~ ~) C~l ~ ~1 ~ C\.l ~ O
H a~ D O O ~ . . 0 ~ O ~O .3 ~1 U`~
~ ~ ~rl O C~l ~i 0 0 cr~ 1 N C\~
r~ H tr- O r-- _~ O O Ir~
r~ H N O U~ i I I I I I I I I I N I r~l O
N ~ ~
H \O O ~ N O 0~ N N H Cl~ N 11~ 0 N N 0 0 \0 O O
O H N O ~1 N ~ ~ ~_1 ~ Ir~ ~ (~J ~r) ~o ~1 ~ o o tY- H O\ ~ O Ll~ l C`;i ri ~ O O C~ ) ~ Hi H H r~i ~ ~0 ~q ~ H H (rl o C'J Lr~ N ,1 0 0 0 a~ ~ ~ ~ ~7 ~1 H O (~ 0 U~ l L~ O O ~ ~ 0 C0 1~ 0 H
0~ H O I I I I r~l N ~ ~i 11~ ~0 0 N ~L) N O C0 O O
N H r~ CC) ~ H t~ O O ~ t~ ~7 0 1~ ~ O O
:~ , ~ o c\~ N ~ o o co O\ a~ ~ w N ~i ~1 ~i ~i ~d ~`
O (I~ +~
d $ ,~
r~ ~
rO~N ^ ~ æ ~ o h o a) _ v O ~Ji R0 ~ir ~ ~ ~æ 3 O O ;~
. h ~ r~ $ C) ,s (V ~ IV
r~ o q~ h ~ æ h $ ~ ~ $
C~ H H ~ ~ rl ~ rl ^ ~d bD C) ~ a C) r~ c~
~i 0 0 ri ~ ~ ~ .rl a ~ h ~ ~ aJ ~ ~ u2 u~ u2 - ~ ~ ~; ~ r~ r~ O ~; ~ r~ r~ ~ rl O rl r~ ~ O
rd 14 ~ 0 0 C~ rl ^ u~ h ,Q ~ ~ ui ~ H ~I r--r~ r~ ~n rl ~ V :~ 0 ~ h ~ a ~ ~ o s~ o r ~ ~ rd ~ ~ ~i r-~ h ~ ~: ~ g a FCi r1 r-i Ha) a) 0 ~ 0 +~ ~ h +~ h ~ U~ h ^ ,1 r1 a) 0 0 0 r~ r1 ~ h ~ F~
o 'O ~ , r~ , ~ ¢ r~ C~ ¢ U~ E-t a~ ~ J 0 ,n ~
O O rd O O ~ri 51 ~ O H r1 rd bD -ri r1 a~ æ ~o c~ ~ ~ h o h i hi ~ 'I h ~ vi ui ~i O H ~ H r~ o o E rd a) ri O ,!~1 vi h ~
O ~i ~ O ~ ~ 5~ d O ,1 ~, O ~ r h O +~ ~
ui ~Li F~i C~~ ~ ~ri C~ a) +~i O ~i O O a~ +~ d O R H
r c~ ~: r~ r~

~ ~8 -FOOT~OTES TO TABLE V

1. Based on a 2:1 mole ratio of Polyol to TDI.
2. This is the product obtained by multiplying the wt.% coupled polyol in the reaction product by the wt.% of the coupled polyol reaction product.
3. The catalyst is azobis(isobutyronitrile).
4. Determined according to the procedure described above using a 200 gram unstripped sample diluted with 400 grams of anhydrous isopropanol and screens of l.ô square inches.
5. This èxample is included for sake of completeness. The results are not considered representative in view of the results shown in Examples 38 and 40~
6. Estimated from monomer feed and expected conversion.

~ ~'7S~
, Samples of polymer/polyol prepared in Examples 29-40 were molded into flexible polyurethane foams in accordance with the procedure previously described. All foams were tested for combustibility, according to MVSS-302, and all foams passed the standards required. Foams samples prepared from polymer/polyols made in accordance with the present invention (viz~ - Examples 38 and 40)9 when diluted to a polymer content of 16 wt.% by addition of further base polyol, did not even burn to the 1-1/2 inch bench mark prescribed by MVSS-302.
With regard to the properties of the polymer/polyols set forth in Table V, the 50 acrylonitrile: 50 styrene polymer/polyols of Examples 30 and 31 exhibit decreased centrifugible solids levels relative to the control, the polymer/
polyol of Example 29. A comparison of the 40 acrylonitrile:60 styrene polymer/polyol control, E~ample 34, with the polymer/polyols of Examples 35-37 shows the tendency of increasing amounts of the coupled polyol in improving the filterability and centrifugible solids level.

These Examples illustrate the preparation of coupled polyols by the in situ method previously described and the use of the resulting coupled polyol reaction product in forming polymer/polyols without further dilution.
The reaction parameters and properties of the polymer/polyols are set forth in Table VI:

-~ 50 ~

O C~ O C~ D ~ O ~O ~ ~ ~ ~ ~ ~
I o . o ~ ~1 ~1 0 0 x ~1 a~ (~ O O ~ ~ D O ~ 0 J o c~ ~ 0 o~ o ~D ~D O\ ~ ~ ~ C~l u~ a u~ ~ o C~J o o ::1' 1 0 O a~ D O O

a:~ L~o ou~ o o I O O ct~ ~ O O O
W N 01 r l t~O (~J u~ l 0 0 CO ~ t~ C`~l N ~ CU
1~ If~O
J o o~ a, o c~:, 1~ t--u~ ~ ~) Il~ t--~ (\I o~ c`J ~ o o o I O O ~1 N ~ Ll~ ~ O
X 'I N C\l H ~ 'I O ('i ~ ~ O C~i O al) ~ ) C\~
C`J
OU~ U~ ~J
I g ~ ~ ~ ~ ~ ~ ~ ~ ~ g ~0 ~ U~ ~ CU ~0 C~J O a~
x ,1 a~ o~ ~ ~ ~ o o ~ . . o ~ ~ ~ ~ ~ u~ ~1 IA

~D ~OD `,~,. oO 0 co co I X ~ ~ ~ ia~ I I i ~ ~ O

U~ O ~ C`J N 1~ N ~0 X O ~D O ~1 ~ ~ ~ ~t r--~ I O co O ~--H O I I I~1 N ~ ~ ~t O ~1 ~ . . . ~ . o ,I r- s~ ,1 ~ o o ~ ~ c~l ,1 ~ o c\~
tYl O C~ C\J ~1 ~1 0 ~ O~ N ~ C~l ~f) O ~ O~
X o 0 o~ U~ ~ r- ~ r- ~ t- ,J ~ ~ o u~ ,1 ,1 o ~ o u~
~OII~ ~C\J~~O~C`J ~O
~I r- o~ o o o r- o~ ,1 o ~ ~ ~ ~ ,1 o t~ ~1 0 ~ :S ~J ~I r1 0 CO ~ ~ N ~1 C`J ~1 ~3 ~1 ~1 0 rl O ~O ~O C\l O
~1 ~ N O O~ O O 0 -1 ~I r- ~ o c~ o ~ o ~D o o O - t-- ~ ~D ~ ~ ~ ~ :r - - - - u~ . o o E~ ~ ~ ~ 0 ~ ~ O O r- a~
li~ ~1 ~I r-l ('') O C\J ~ '~J ~I r l O CO ~ 0 N C\l ~
~1 a~ o ,~ O
~` I O O ~ ,~ ~ No ~ Lr~ ~ N, 0 ~ o ,3 ~ O C\i ,~ ~I r l ~1 0 N Ir~ N r1 0 0 0 ~ 0~ N N ~

O ~ +~ P~ h h $
O ` ~ g g~
q~ _ +, p, h h h C~ 1~ ~ $ ~ ^ h .C
a~J N ~ ~ ' ^ ~c R O N
h ~ ~ q~ ~ ~ o Ir~ r-l O ~ $ O ~ ~ ~1 ~ $ ~J ~ ~
rl ~ e. O ~ h ~J 'V ~ h 3 ~ ~ 3 rC S
0 ~ a O O ~rl a~ ~ ~rt ~ h h ~ h ~D ~ O
~ h ~ rO rO ~ æ ~ ~ +~ a) $ ~ h ~ ~ ~ ~ O
~ ~ ~1 +~ 0 ~ O ~I h ~ O O ~I r-E~ ~ o~ ~ 5 ~ llh~ ~ , h Z ¢ ~ C~
--l ~1 ~1 ~ a) O ~ C) ~ ~ h -1~ h ~ h ^ ~rl O
O O O r~ l ~ h ~ R ~ h ~d U +~ 5 . . o , ~ ~1 +~
r-l ~ O O ~ rt æ o o ~ o o ~r~td ~ + a~ + ~ o O ~ h O h ~
~-1 a) a) ~ t~ tæ o CJ ~ h X ~ ~rl h o~ ~ ,~ r~ o o ri ~ a) ,~ o ~I h O
c~ ~ O +~ +~ h rJ C) ~ O ~r1 ~ O ~r1 ~ ~d h O ~ +~ ~
~ r~ m" ~ a ~ O ~ ,~
r~ ~d ~; ~ ~ r r~ ~ m o ~

~ 51 -1. Based on a mole ratio of polyol: isocyanate as set forth in Table IV.
2. This is the product obtained by multiplying the wt.% coupled polyol in the reaction product by the ~t.% of the coupled polyol reaction product.
3. The catalyst is azobis(isobutyronitrile).
4. Determined according to the procedure described above using a 200 gram unstripped sample diluted with 400 grams of anhydrous isopropanol and screens of 1.8 square inches.
5. Measured.
6. Estimated from monomer feed and expected con~ersion.

Samples of polymertpolyol prepared in Examples 41-50 were molded into flexible polyurethane foams in accordance with the procedure previously describedO All samples were then tested for combustibility as described in conjunction with Examples 29-40. All samples met the standards required. The samples made from the polymer/polyols of Examples 46 (diluted to reduce the polymer content to 21 wt.%), 47 and 50 did not even burn to the 1-1/2 inch bench mark prescribed.
A comparison of the viscosities of the in situ produced coupled polyols with the viscosities of the coupled polyol reaction products made in prior Examples (diluted to the same coupled polyol level) show the tendency for somewhat lower viscosities obtained with the in situ technique.
Further, the reduction in polymer content to about 20 wt.% (in comparison to the higher level in Examples 20-29) allowed preparation of polymer/polyols of quite satisfactory stability at acrylonitrile to styrene weight ratios ranging from 50:~0 to 30:70.

This Example illustrates the preparation of a polymer/polyol with a relatively high polymer content.
The reaction parameters and properties of the polymerJpolyol are set forth in Table VII:

r ~ 53 ~

TABLE VII
Example No. Sl Base Polyol Blend:
8ase Polyo1 Type X
Base Polyol wt.% 93 Coupled Polyol Reaction Product Ex. 19 wt.% 7 Wt.% Coupled Polyoi in reaction productl 95~2 Wt.X Coupled Polyol in Blend2 6.7 Brookfield viscosity at 25C~ cps 558 Calc. Hydroxyl Nn., mg KOH/gm 49.3 Reaction Temperature, C 125 Catalyst conc., wt.% of total feed3 0.50 Monomer + catalyst, wt.% of total feed 34~41 lS ~atio of Acrylonitrile/Styrene (wt/wt) 72/28 Polyol feed rate, gm/hr. 1828 Monomer + catalyst, feed rate (gm/hr) 959 Residual: Acrylonitrile, wt.% 1~29 Styrene, wt.% O.lS
TMSN3 wt.% 0.17 Conversions: Acrylonitrile, wt.~ 94~8 Styrene, wt.% 98~2 Combined 9 wt.X 95. 7 Total Polymer, wt.%, by calc. 33~48 Hydroxyl No.~ mg KOH/gm 32~ 77 Brookfield ~iscosity at 25C~ No. 3 spindle/
12 rpm, cps 2840 Centrifugible Solids, wt.%4 7~89 Filterability, 150 mesh, ~ through screen 100 700 mesh, % through screen 100 _ 1. Based on a 2:1 mole ratio of polyol to TDI.
2~ This is the product obtained by multiplying the wt.X coupled polyol in the reaction product by the wt.~ of the coupled polyol reaction product.
3. The catalyst is azobis(isobutyronitrile).
4. Determined according to the procedure described above using a 200 gram unstripped sample diluted - with 400 grams of anhydrous isopropanol and screens of 1.8 square inches.
.

As can be seen, the polymer content of the polymer/polyol is calculated to be over 33 percent by weight, the filterability characteristics are excellent and the centrifugible solids level acceptable.

L~

Thus, as has been seen, the present invention provides a method for preparing stable polymer/polyols by a facile synthesis not requiring any substantial economic penalty. Utilizing this invention, polymer/polyols can be made with extremely high polymer contents for use in applications requiring high load capabilities.
Further, stable polymer/polyols can be prepared which are capable of conversion ~o virtually scorch-free, slab-stock foam at densities lower than 1075 pounds per cubic foot~ Indeed, employing some formulations, polyurethane foams can be made that satisfy even highly rigorous interpretations of desired combustibility resistance, as determined by MVSS-302, t.he standard for foam used in motor vehicle applications.
The desirability of the present invention resides in the fact that such facile preparation of stable polymer/polyols is achieved without the need to resort to the inclusion of materials likely to be harmful to desired polyurethane characteristics.
More specifically, the formation of the coupled polyols utilized in this invention simply carries out reactions that would eventually occur upon conversion of the polymer/polyol to a polyurethane, reordered in a time sequence to achieve the considerable benefits described herein. This is in marked contr~st to prior techniques which either do not allow a facile preparation of the polymer/polyol ~ in the first instance, or require the inclusion of materials that will impart adverse effects when such polymer/polyols are converted to polyurethanes.

Claims (23)

WHAT IS CLAIMED IS:
1. A normally liquid, stable polymer/polyol composition formed by polymerizing, in the presence of a free radical catalyst, (1) from about 10 to about 50 weight percent of a mixture of acrylonitrile and an ethylenically unsaturated comonomer or comonomers in a weight ratio, respectively, of from about 80:20 to about 20:80, dissolved or dispersed in (2) from about 50 to about 90 weight percent of a polyol mixture comprising (a) a base polyol having a number average molecular weight of at least about 500 and (b) a coupled polyol consisting essentially of the reaction product of a polyol having a functionality in excess of 2 reacted with a polyisocyanate in such proportion that the ratio of hydroxyl groups to isocyanato groups is greater than 1, the coupled polyol being present in an amount sufficient to stabilize the resulting polymer/polyol.
2. The polymer/polyol composition of claim 1 wherein styrene is the comonomer and the weight percent of the mixture of acrylonitrile and styrene is in the range of from about 30 to about 40.
3. The polymer/polyol composition of claim 2 wherein the weight ratio of acrylonitrile to styrene is in the range of from about 80:20 to about 50:50.
4. The polymer/polyol composition of claim 1 wherein styrene is the comonomer and the weight ratio of acrylonitrile to styrene is in the range of from about 40:60 to 20:80.
5. The polymer/polyol composition of claim 1 wherein styrene is the comonomer and the weight ratio of acrylonitrile to styrene is in the range of from about 30:70 to 20:80.
6. The polymer/polyol composition of claim 1 wherein the base polyol is a poly(oxypropylene) polyol.
7. The polymer/polyol composition of claim 6 wherein the poly(oxypropylene) polyol has a nominal functionality in the range of from about 3 to about 4 and a hydroxyl number of from about 25 to about 70.
8. The polymer/polyol composition of claim 1 wherein the polyol reacted with the polyisocyanate to form the coupled polyol has a functionality in the range of from about 2.5 to about 4.
9. The polymer/polyol composition of claim 8 wherein the polyisocyanate is toluene diisocyanate.
10. The polymer/polyol composition of claim 1 wherein the polyisocyanate is toluene diisocyanate.
11. The polymer/polyol composition of claim 1 wherein the ratio of hydroxyl groups to isocyanato groups is 2:1 or greater.
12. The polymer/polyol composition of claim 1 wherein the coupled polyol, based upon the total weight of the base and coupled polyols, is present in an amount of from about 5 to about 50 weight percent with the mole ratio of the polyol constituent of the coupled polyol to the polyisocyanate being about 2:1.
13. The polymer/polyol composition of claim 1 wherein the polyol reacted with the polyisocyanate is identical to the base polyol.
14. A process for producing a normally liquid, stable polymer/polyol composition which comprises: (a) providing a polyol mixture comprising (1) a base polyol having a number average molecular weight of at least about 500 and (2) a coupled polyol consisting essentially of the reaction product of a polyol having a functionality in excess of 2 reacted with a polyisocyanate in such proportion that the ratio of hydroxyl groups to isocyanato groups is greater than 1, (b) dissolving or dispersing from about 10 to about 50 weight percent of a mixture of acrylonitrile and a comonomer or comonomers in a weight ratio, respectively, of from about 80:20 to about 20:80 in from about 50 to about 90 weight percent of said polyol mixture, and (c) polymerizing the mixture of acrylonitrile and styrene dissolved or dispersed in said polyol mixture in the presence of a free radical catalyst, said coupled polyol being present in an amount sufficient to stabilize the resulting polymer/polyol.
15. The process for producing the normally liquid, stable polymer/polyol composition of claim 14 wherein said coupled polyol is formed in situ in the base polyol by addition thereto of an amount of said polyisocyanate sufficient to form the required proportion of coupled polyol prior to step (b).
16. The process for producing the normally liquid, stable polymer/polyol composition of claim 15 wherein styrene is the comonomer and the weight percent of the mixture of acrylonitrile and styrene is in the range of from about 30 to about 40.
17. The process for producing the normally liquid, stable polymer/polyol composition of claim 16 wherein the weight ratio of acrylonitrile to styrene is in the range of from about 80:20 to about 50:50.
18. The process for producing the normally liquid, stable polymer/polyol composition of claim 15 wherein styrene is the comonomer and the weight ratio of acrylonitrile to styrene is in the range of from about 40:60 to about 20:80.
19. The process for producing the normally liquid, stable polymer/polyol composition of claim 15 wherein styrene is the comonomer and the weight ratio of acrylonitrile to styrene is in the range of from about 30:70 to about 20:80.
20. The process for producing the normally liquid, stable polymer/polyol composition of claim 15 wherein the base polyol is a poly(oxypropylene) polyol.
21. The process for producing the normally liquid, stable polymer/polyol composition of claim 20 wherein the poly(oxypropylene) polyol has a nominal functionality of from about 3 to about 4 and a hydroxyl number of from about 25 to about 70.
22. The process for producing the normally liquid, stable polymer/polyol composition of claim 15 wherein the polyisocyanate is toluene diisocyanate.
23. The process for producing the normally liquid, stable polymer/polyol composition of claim 15 wherein the coupled polyol is present in an amount of from about 5 to about 50 percent, based upon the total weight of the base and coupled polyols.
CA000412105A 1981-10-02 1982-09-24 Polymer/polyols, methods for making same and polyurethanes based thereon Expired CA1179440A (en)