CA2026944A1 - Ceramic welding process and lance for use in such process - Google Patents

Ceramic welding process and lance for use in such process

Info

Publication number
CA2026944A1
CA2026944A1 CA002026944A CA2026944A CA2026944A1 CA 2026944 A1 CA2026944 A1 CA 2026944A1 CA 002026944 A CA002026944 A CA 002026944A CA 2026944 A CA2026944 A CA 2026944A CA 2026944 A1 CA2026944 A1 CA 2026944A1
Authority
CA
Canada
Prior art keywords
gas
outlet
curtain
particles
lance
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Abandoned
Application number
CA002026944A
Other languages
French (fr)
Inventor
Pierre Robyn
Alexandre Zivkovic
Leon-Philippe Mottet
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
AGC Glass Europe SA
Original Assignee
Glaverbel Belgium SA
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Glaverbel Belgium SA filed Critical Glaverbel Belgium SA
Publication of CA2026944A1 publication Critical patent/CA2026944A1/en
Abandoned legal-status Critical Current

Abstract

ABSTRACT

CERAMIC WELDING PROCESS AND
LANCE FOR USE IN SUCH PROCESS

A ceramic welding process which facilitates the formation of high quality erosion-resisant and corrosion-resistant refractory weld masses comprises projecting against a surface (1) an oxidisable mixture of refractory particles and particles of a fuel material in a carrier gas (7) which contains at least sufficient oxygen for substantially complete oxidation of the fuel particles, whereby sufficient heat is released for at least surface melting of the projected refractory particles and a ceramic weld mass is formed against said surface (1) under the heat of oxidation of the fuel particles, wherein at least one additional stream of gas (9) is projected against said surface (1) so as to form a substantially continuous gas curtain surrounding said carrier gas stream(s).
The invention also provides apparatus to effect the ceramic welding process, comprising a lance (5) having a first outlet (6) for the discharge of such ceramic welding powder in a carrier gas (7) along a discharge path towards the surface (1), and a second outlet (8) for the discharge of gas to form the substantially continuous gas curtain.

Description

CERAMIC WELDING PROCESS AND
L~NCE FOR USE IN SUCH PROCESS

This invention relates to a ceramic welding process and to a lance suitable for use in such a process.
Previous ceramic welding processes have been described in Glaverbel's British Patents Nos 1,330,894 and 2,170,191.
S Ceramic welding is particularly suited to the in situ formation of a refractory mass on a refractory wall of furnaces or o~her refractory apparatus for the hot repair of the wall. It is preferably implemented when the wall is substantially a~ its normal operating temperature. It is particularly useful for repairing or reinforcing the walls or wall linings 0 of glass melting furnaces, coke ovens, cement kilns or fumaces used in the petrochemica~ industry, or refractory apparatus used ~n ferrous or non-ferrous metal metallurgy. Moreover, the repair can sometimes be carried out during the operation of the furnace, for instance for the repair of a glass melting furnace superstructure, or dunng the normal 1~ operating cycle of the refractory article, for example a steel-pouring ladle can sometimes be repaired within ~he norrnal interval between teeming -and recharging. The process is also useful for the formation of refractory cornponen~s, for instance for the sur~acing of other refractory substrates.
In the ceramic welding process as practised, a mixture of refractory particles and fuel particles (the "ceramic welding powder") is conveyed from a powder store along a feed line to a lance from which it is projected against a target surface. The carrier gas which leaves the lance outlet with the ceramic welding powder ("the carrier gas") may be pure (commercial grade) oxygen, or it may comprise a proportion of a subst~ially inert gas such as nitrogen, or indeed some other gas. In any event, the carrier gas leaving the lance outlet with the ceramic welding powder contains at least sufflcient oxygen ~or substantially complete combustion of the fuel particles. It is by no means essential 2 ~ ,d~

that the gas stream into which the welding powder is introduced from the feed store should have the same composition as the carrier gas which leaves the lance outlet. Some, or indeed all, of the required oxygen in the carrier gas may be introduced into the feed line at one or 5 ~nore locations be~ween the powder introduction point and the outlet of the lance. The fuel used essentially consists of particles of a material which is capable of being oxidized exothermically to form a refractory oxide product. Examples of suitable fuels are silicon, aluminium, magnesium, zirconium, and chromium. Such metallic fuels may be 0 used alone or in cornbination. 1~e fuel burns and heat is liberated by its combustion to melt at least the surfaces of the refractory particles so that a strongly coherent refractory weld mass is formed which adheres well to the target surface.
It is common practice to select the ceramic welding powder in 5 such a way that the weld deposit formed has a chernical composition which is approximately the same as that of the target surface. l'his assists in reducing thermal shock at the interface behveen a repair weld and ~e repaired refractory due to temperature cycling of the furnace.
Such selection of the welding powder also helps to ensure that the 20 refractory quality of the weld mass is suf~iciently high for the location where that repair is made. Of course it is also known to select ~e ceramic welding powder in order to form a repair or lining of higher grade than the refractory Oll which the weld is fo~ned.
When folming a refractory mass by ceramic welding, a certain 2s amount of porosity may be incorporated in the weld mass. The extent of such porosity is dependent in part on the skill of the welder, and on the conditions under which the welding operation is carried out. Such porosity may be tolerable, indeed in some circumstances it may be advantageous, since a high degree of porosity promotes thermal 30 insulation. However, an excessive degree of porosity may be objectionable at furnace locations where the refractory is subjected to particularly severe corrosive action, and especially the corrosive or erosive action of molten material contained within the furnace. ~he degree of porosity which is acceptable in a given piece of refractor.v material depends on the inherent refractoriness of that material and on S the conditions to which it will be subjected in use.
The present invention results from research into the formation of a refractory lining or repair on parts of apparatus which are particularly likely to undergo intense erosion. This erosion may be due in particular to mechanical or thermo-mechanical abrasion, or to liquid or o gaseous phase corrosion of the material forming the wall, or may be due to a combination of these effects.
One example of such a requirement for good resis~ance to a tendency to in~ense erosion is in the field of glass melting furnaces.
The inner surface of the tank blocks of a glass melting urnace at the 5 locatiorl of the sur~ace of the molten glass bath provides a particular example of a refractory surface subject to very intense corrosive action. The tank block surface erodes very rapidly to such an e~tent that half the thickness of the blocks may be readily and compara~ively rapidly eaten away at this location. This erosion is known by the 20 technical term "flux line corrosion". Tank blocks subject to very high temperatures, such as the tank blocks of the melting and refining zones of the furnace, are conventionally formed of highly re~ractory materials such as refractory materials containing a high proportion of zirconia.
Even so, they have to be continuously and vigorously cooled to lessen 25 the erosion.
Other exarnples of refractories which are subject to risk of particularly severe erosion are casting orifices or ladles used in the manufacture or transport of molten metals, for example torpedo ladles, as used for instance in the iron and steel industry, copper smel~ng and 30 refining furnaces, converters such as those used in steelmaking or in the non-ferrous metals industry. Cement kilns may also be mentioned here.

4 2~

It is a principal object of this invention to provide a new ceramic welding process which facilitates the fo~nation of high quality refractory weld masses which exhibit good resistance to erosion and corrosion.
According to this inverltion, there is provided a ceramic welding process in which a ceramic welding powder comprising a mixture of refractory p. rticles and particles of a fuel material which is capable of being oxidized to form a refractory oxide is projected aga~nst a surface in one or more strecuns of carrier gas which contains at least sufficien~
0 oxygen for substantially complete oxidation of the fuel particles, whereby suf~lcient heat is released for at least surface melting of the projected refractory particles and a ceramic weld mass is formed against said surface under the heat of oxidation of the fuel particles, characterised in that at least one additional strearn of gas is projected against said surface so as to form a substantially continuous gas curtain sulTounding said carrier gas stream(s).
It is rather surprising that the blowing of additional gas in this way should have the beneficial effect which it does, of allow~ng the formation of ceramic welds of high quality with good resistance to erosion and corrosion more easily and more consistently than before.
The achievement of a high quality weld by a method of the inven~on is less dependent on the skill of the individual welder ~an when forming a weld by a process in which the gas curtain is omitted but which is otherwise similar. We attribute this result to the fact that welds made by a process according to this invention tend to have a lower porosity than welds made by a process in which the gas curtain is omitted but which is otherwise similar.
The reasons why this beneficial effect should be achieved are not clear. One possibility is that the gas curtain isolates the ceramic welding reaction zone from the arnbient furnace atmosphere, so preventing that a~nosphere from having any adverse effect on those .

2 ~ s ~

reactions, and preserving unifo;m working conditions at tne reac~ion zone. Another possibility is tnat the gas curtain may have a quenching effect in reducing the temperature of the just-formed, still soft refractory deposit which may prornote a favourable cooling and 5 crystallization of the weld material. This may in turn act to reduce the propensity for gas which may becorl1e dissolved in the incipient ceramic weld mass while it is at least partially molten to form pores, so that any pores which are formed within the weld are of smaller size and thus less objectionable. However tnis theory goes against currently received 0 wisdorn in the art according to which it is not desirable for rapid cooling to take place in order to avoid problerns of stratification due to innomogeneities at bo~mdary layers of material deposited by successive passes of the welding lance over the target surface.
The method of the invention is also surprising in that it would ~s have been expected, in view of the difficulty of controlling the operating conditions, that tne spraying of a gas curtain around the carrier gas stream and thus around the zone where the ceramic welding reactions take place and where the ceramic weld deposit is formed, would interfere with the exothermic reaction leading to the formation of 20 the weld.
It has to the contrary been observed in practice that the projection of a gas curtain provides a supplementary parameter for controlling the different elements which come into play in the reaction zone in order to form the refractory mass during the performance of the method of the 2s invention. This conseguently provides a supplementary control parameter acting on the evolution of the exotherrnic reac~ion, thereby allowing improved control of the formation of the refractory weld mass.
It has also been observed that the gas curtain makes it possible to reduce the influence of the surrounding environmen~ on the reaction 30 zone. The reaction zone is consequently better protected from any turbulence which may exist in ~e surrouncling atmosphere. Thus for example, in a common case where the process is used during the ~J~ J~

operation of the furnace, the reaction zone is made more independent of interference resulting for instance from the switching on or off of a burner in the vicinity of the operating location.
The gas curtain also makes it possible more readily to confine the s particle mixture in the reaction zone so as to concentrate and intensify the cerarnic welding reaction and thus lead to the forrnation of a refractory rnass of high quality. The gas curtain assists in co~ming the projected refractory material and the fuel combustion products to the reaction zone so that they are readily incorporated into the weld mass 10 forrned. The incorporation of such combustion products into the refractory mass forrned is no disadvantage in a ceramic welding process since those products are thernselves refractory oxides.
The gas curtain may be projected from a multiplicity of outlets arranged in a ring around the powder discharge outlet(s). Of course such outlets would require to be closely spaced in order to produce a substantially continuous curtain. Preferably, howeYer, the gas curtain is projected as an annular stream. The use of a continuous annular outlet for projecting an annular curtain stream promotes the efficiency of the Cllrtaill and can also allow a sirnpler construction of apparatus for 20 perfo~ing the process of the inYention. A protective sheath is thus formed around the carrier gas stream thereby making it possible to prevent rnaterial, in particular gases, from the surrounding atmosphere from being drawn into the carrier stream containing the oxidizing gas and the particle mixture. The whole region of the exotherrnic reaction 2s and the spraying of ~he mixture in its oxidizing carrier gas can thus be isolated from tne surrounding environment so as to prevent the introduction of any element foreign to and interfering wit'n the exothelmic reaction and the latter can consequently be better controlled.
In order to form the most efficient gas curtain aroung ~e carrier 30 gas and entrained particles, the curtain gas should be ejected from one or more outlets which is or are spaced from the ca~Tier gas outlet(s) but the different outlets should not be too widely spaced. The optimum spacing depends to a large extent upon the size of the carrier gas outlet(s).
Some preferred embodiments of the invention are primarily intended for small to moderate scale repairs, or situations where larger s repairs are needed but the time available for repair is not critical, and the particles are projected from a lance having a single carrier gas outlet having a diarneter of between 8rnm and 25mm. The cross sectional area of such outlets will thus be between 50 and 500 rnm 2. Such lances are suitable for projecting ceramic welding powder at rates of 30 0 to 300 l~g/h. In some such preferred embodiments wherein the carrier gas is ejected ~rom an outlet having an area of between 50 and 500 mm2, the gas curtain is ejected from one or more outlets spaced from the calTier gas outlet by a distance of between 5 and 20 mm.
Other pre~erred embodiments of the invention are primarily S intended for large scale repairs which must be effected in a short time, and ~e particles are projected from a lance having a carrier gas outlet having a cross sectional area of between 300 and 2,300 rnm 2. Such lances are suitable for projecting ceramic welding powder at rates of up to 1000 kg/h, or even more. In some such preferred embodLments 20 wherein the carrier gas is ejected from an outlet having an area of between 300 and 2,300 mm2, the gas curtain is ejected from one or more outlets spaced from the carrier gas outlet by a distance of between 10 and 30 rnm.
The adoption of one or other of these spacing ranges between the 2s carrier gas and the curtain gas outlets promotes the formahon of a clear and defimite barrier between the ceramic welding reaction zone and the ambient atmosphere while allowing substantially avoidance of any interference between the dif~erent gas s~reams by ensuring ~at they remain substantially separate until they are deflected at the target 30 surface.

J

Advantageously, the volurne rate of discharge of the curtain gas is at least half the volume rate of discharge of the carrier gas. The adoption of this feature facilitates the formation of a thick and effective curtain. The discharge rate of the curtain gas may for example be at least two-thirds of the discharge rate of the carrier gas. or it may even be higher than the carrier gas discharge rate.
Preferably, the discharge velocity (calculated at normal pressure) of the curtain gas is greater than one fifth of the discharge velocity of the carrier gas. We measure gas volume discharge rates in normal o cubic metres per hour, and gas discharge velocities are calculated from this volume discharge rate and the area of the outlet(s) from which the gas is discharged on the assurnption that the gas pressure in the stream is normal at the momellt when it leaves its outlet. l'he adoption of this feature allows the formation of an effective gas curtain. For the best results, we have found it preferable that the discharge velocity (calculated at normal pressure) of the curtain gas should be between one fifth and ~ree fifths of the discharge velocity of the carrier gas. The adoption of this feature allows a low disturbance of the flow pat~ern of the canier gas s~eam and of matenal in the ceramic welding reaction zone. The adoption of this feature further entails that there is a less abrupt gas velocity gradient ~rom the carrier gas stream(s) to the arnbient atmosphere than would otherwise be the case, and this is found to promote weld quality, perhaps because there is less dilution of the carrier gas stream and its entrained particles.
In some prefe~ed embodiments of the invention, the gas s~earns are discharged from a lance which is cooled by fluid circula~ing through it. Such cooling may easily be achieved by providing the lance with a water jacket. Such a water jacket may be located to su~round a central tube or tubes for the feed of carrier gas and ceramic weld~ng powder~

while being itself surrounded by an annular passage ~or the conveyance of curtain gas. The water jacket may easily be constructed to a thickness which is such as to ensure any desired spacing between the carrier gas outlet~s) and the curtain gas outlet. Alternatively, or in addition, there may be a water jacket which surrounds all the gas discharge tubes of the lance. In either case, the temperature of the curtain gas discharged will be, in general, and when considering the repair of furnaces at substantially their operating temperature, considerably lower than the environmental temperature within the 0 furnace, and it may be at a temperature which is broadly similar to that of the carrier gas.
To do this runs wholly against conventional practice in the art of ceramic welding. One of the permanent concerns when carrying out ceramic welding is to prevent the temperature at the impact zone on the target surface from being too low during the formation of the refractory mass, for instance as a result of inadequate control of the various exothermic reaction parameters. An impact zone which is too cold may for instance lead to momentary interruptions of the exothermic reaction. It is in particular known that this temperature leads, if it is too low, to ~e forma~ion of an irregular and uncontrolled porosity in the refractory weld mass formed so that it is rather porous and has little resistance to abrasion or corrosion. This porosity is particularly evident if the refractory mass is formed by several passes of the spray lance.
2s When the impact zone is displaced over the surface to be ~sated, at least part of this relatively cool gas~ in a qu~tity sufficieIlt to form an effective shield a~ound tne impact zone, tends to cool the surface being trea~ed just prior to the impact of the welding material. This is not recommended at all in most welding techniques if an accep~able result is to be achieved. That there is advantage in spraying, accordLng to this preferred feature of the invention, a cooled gas curtain agains~ the ~J f~

surface of the substrate around the impact zone is completely surprising. Such a gas spray will tend to have a strong cooling effect on the impact zone and it would therefore be expected that this cooling would lead to the formation of a porous mass with little resistance to S erosion.
Notwithstanding this, however, we have observed experimentally that, in a completely unexpected manner, the supplementary control parameter for the exothermic reaction provided by the adoption of the invention allows the formation of dense refractory masses more 10 resistant to erosion than the masses ~ormed in the past by cerarnic welding methods, and in particular it does so when use is made of a cooled lance. This result is very surprising since it runs counter to the - opinion which people skilled in the art have held in this field for many years. -The porosity of the refractor,v mass formed is one of the essential factors in deterrnining its level of resistance to erosion. Porosit,v inherendy weakens ~e structure of the refractory mass. Furthermore, the pores provide access routes for the erosive medium thereby making the refractory material more sensitive to erosion since the erosive 20 medium can act within the interior of the mass.
There is also another consideration to be taken into account.
Clearly, the projected refractory particles have to be heated to melt at least their surfaces in order to fo~n a homogeneous weld mass, and the target surface rnust also be strongly heated to allow the best bond 25 between the deposit and that surface. However, if the temperature at the target region is too high, there is a risk that the deposit will be too fluid to remain in position. This risk is oiF course hig~er on vertical or overhanging target surfaces. The risk is also greater the more vigorous is the ceramic welding reaction which takes place at the working si~e.
30 - Such a vigorous reaction may however be essential in order sustain the ceramic welding reactions, or to heat the target surface sufficiently for a ~J ~ ~f ~

good bond to be formed between the ceramic weld deposit and that surface, especially if the temperature of the target surface is not very high. We have in mind here temperatures below for example about 700C. Such temperatures may be encountered in furnaces or kilns for s processes carried out at only moderately high temperatures such as cement kilns or chemical reaction vessels. It has been observed in practice that the projection of a relatively cool gas curtain provides a means of controlling the temperature of the impact zone. It is thus easier to prevent the refractory mass being formed from flowing as a 0 resul~ of a high temperature in the impact zone. It is then possible to adjust the various parameters to create a very vigorous exo~errnic reaction to give reliable operation of the process and the formation of a good bond between the deposit and the target surface, even when the latter is not at a very high temperature, while cooling the impact zone to prevent the mass being formed from flowing. This facilitates the achievement of an homogeneous weld.
The cooling effect of the curta~n stream can also have a further important effect in influencing the crystalline form which the weld mass assumes as it solidifies, and this can afford considerable benefits. By way of example, molten rnixture of silica and alumina tend to form mullite when they are allowed to cool slowly: if on the other hand rapid cooling takes place, the alumina crystallizes out as corundum which can be held in a silica phase without the formation of mullite. This too can promote the resis~.ce tO erosion of the weld mass formed.
2s There are various gases which may be projected in order to form the required gas curtain, and the optimum choice of gas will depend on circumstances. VVhile very good results can be achieved using carbon dioxide or nitrogen for forming the gas curtain, some prefer,red ernbodiments of the invention provide that the curtain gas comprises oxygen. For example air may be used since it is inexpensive and widely available. However, the use of commercial grade oxygen ;,J if ~ t i ,~J f,~",, may be preferred: such oxygen will ordinarily be present for the performance of the ceramic welding operation anyway, and it is more efficient for the puIpose in view. If the gas c~lrtain compAses oxygen, it can provide a further oxygen reservoir in the immediate vicinity of 5 the ceramic welding reaction zone, and this facilitates complete combustion of the fuel particles used. This promotes homogeneity within the cerar~Lic weld mass, and it occasionally allows the proportion of the fuel in the ceramic welding powder mixture to be reduced slightly. However, it will be borne in rnind that the carrier gas itself 0 contains at least sufficient oxygen for substantially complete combustion of the fuel and accordingly, as has been stated, the use of an gas such as carbon dioxide or nitrogen which is substantially free from available oxygen does give beneficial results.
Indeed in certain special circumstances, the use of such a gas may be optimal. Some classes of refractory material contain par$icles of an oxidizable material such as carbon or silicon with a view to militating against the diffilsion of oxygen through the refractory, or for other purposes, for example basic magnesia refractories containing up to 10%
by weigh~ carbon particles are used in the steel industry for certain converters. If it becornes necessary to repair such a refractory, it is desirable to ensure that the repair also contains a certain proportion of oxidizable material. Such a repair can be effected by a ceramic welding technique. Such a technique forrns the subject of Glaverbel's Bri~ish Patent Specification No 2,190,671.
Thus in some prefelTed embodiments of the invention, ~he particles discharged in the camer gas stream include particles of an oxidizable material which is $o be incorporated as such in the weld mass and the curtain s~eam is substan~ally free from available oxygen. The adoption of ~is feature has the effect of substantially preverlting the en~ainment of additional oxygen, whether from the gas curtain or ~e arnbient atmosphere, into the incipient weld mass at the reaction zone, and this can inhibit combustion of such oxidizable material so that the yield of oxidizable material left as such in the weld mass deposited is increased.
~dvantageously, ~he fuel material comprises one or more of the s materials in the group consisting of: alurn~nium, silicon, magnesium, zirconiurn and chrormium. Such materials are all capable of being burnt to yield intense heat and form refractory ox~de. Such elements may be used alone or in admixture as required. Furthermore, alloys of such materials may be used. The alloying of an element which 0 combusts very easily and rapidly with one which is more reluctant to combust ensures an intimate mixture of those elements, and by suitable selection of the alloy constituents, a more stable reaction which proceeds at a more desirable reaction rate can be achieved.
~ dvantageously, at least 50% by weight of the ~uel particles have a grain size less than 50 ,um, and preferably, at least 90% by weight of the fuel particles have a grain size less than 50 ~lm. The average grain size may for example be less than 15 ~m, and their maximum grain size less than 100 ~n and preferably less than 50 ~Lrn. The fuel particles ~us oxidize readily thereby facilitating the development 20 of intense heat energy in a small space and the achievement of a good weld between the particles of refractor,v material. The small size of these fuel particles also promotes their complete combustion and consequently the llomogeneity of the mass formed.
Preference is given to the formatiorl of ceramic weld masses of 25 particularly high refractory quality, and to that end it is preferred that atleast the greater part by weight of the re~ractory particles projected - consists of alumina and/or zirconia, or of magnesia and/or alumina.
The invention extends to a cer~nic weld mass when formed by a process according ~o the invention, and it also includes apparatus 30 specially adapted for ~e per~ormance of the process.

, Accordingly, the present invention includes a lance comprising an outlet for the discharge of a ceramic welding powder in a carrier gas along a discharge path towards a surface for the performance of a ceramic welding process, characterised in that such lance comprises a 5 second outlet or group of second outlets, for the discharge of gas, said second outlet or outlet group being so shaped and arranged and so spaced both axially and radially in relation to the powder outlet that gas can be discharged from said second outlet or outlet group so as to form a substantially continuous curtain surrounding and generally parallel to 0 the powder discharge path.
The lance of the invention is simple and makes it possible readily to form a gas curtain around the zone of the impact of the carrier gas stream and entrained powder discharged from the powder outlet. This lance of the invention provides the welding operator with a 15 supplementary control parameter allowing him to achieve a high-quality ceramic weld.
The curtain gas may be discharged from a group of spray orifices disposed around the powder outlet, but preferably, such second outlet for the discharge of curtain gas is a con~nuous annular outlet. This is a 20 simple, easy and effective way of maintaining a gas curtain around ~e calrier stream comprising the oxidizing gas and ~e particle rmixture.
Such annular outlct need not be strictly circular. Indeed it may have a rectangular shape if desired.
In order to ~orm the most efflcient gas curtain around the carrier 25 gas and en~ained particles, the curtain gas should be ejected from one or rnore outlets which is or are spaced from the carrier gas outlet(s~ bu~
the different outlets should not be too widely spaced. The optimum spacing depends to a large extent upon the scale of operations in which the lance is intended to be used.

Some lances according to the invention are primarily intended for srnall to moderate scale repairs, or where time is not a critical factor, and the lance has a carrier gas outlet having a diarneter of between 8mm and 25mm, or an outlet group having a comparable aggregate outlet area. The (aggregate) cross sectional area of such outlets will thus be between 50 and 500 mm2. Such lances are suitable for projecting ceramic welding powder at rates of 30 to 300 kg/h. In some such preferred embodiments wherein such powder outlet has an aggregate area of between S0 and S00 mrn 2, the or each said second outlet is spaced from the powder outlet by a distance of betwèen 5 and 20 mm.
O~er lances according to the i~vention are primarily intended for large scale or rapid repairs, and ~e lance has a single carrier gas outlet or a group of ca~Tier gas outlets having a cross sectional area of between 300 and 2300 mm2. Such lances are suitable for projecting cerars~ic welding powder at rates of up to 1000 kg/h, or even more. In some such preferred embodiments wherein such powder outlet has an aggregate area of between 300 and 2300 mm 2, the or each said second outlet is spaced from the powder outlet by a distance of between lO and 30 mm.
The adoption of one or other of these spacing ranges between the carrier gas and the curtain gas outlets promotes the formation of a clear and definite barrier between the ceramic welding reaction zone and the ambient atmosphere while allowing substantially avoidance of any interference between the different gas strearns.
In some preferred embodiments of the invention, such lance incorporates a jacket adapted for the circulation of coolant. The preferred coolant is water in ~iew of its thermal capacity and ready availability. Such a water jacket may be located to sulTound a central tube or tubes for the feed of carner gas and ceramic welding powder, while being itself surrounded by an annular passage for the conveyance $~ J~

of cur~ain gas. The water j2cket may easily be constructed to a thic}~less which is such as to ensure any desired spacing between the carrier gas outlet(s) and the curtain gas outlet. Alternatively, or in addition, there may be a water jacket which su~rounds all the gas s discharge tubes of the lance. In either case, the temperature of the curtain gas discharged will be, in general, and when consideling the repair of furnaces at substantially their operating temperature, considerably lower than ehe environmental temperature within the furnace, and it may be at a temperature which is broadly similar to that 0 of the carrier gas.
The advantageous ef~ect this has on the formation of a ceramic weld mass has already been explained. In addition to ~at, the provision of a cooling jacket rneans that the lance may remain in a high temperature environment such as that within a furnace or other refractory structure at its operating temperature for considerable periods of time without becorning overheated. This has advantages for operational reasons, and it also helps to prolong the useful life of the lance.
Preferably, the area of the second outlet or outlet group is between two thirds of and three times the area of the powder outlet. Such a second outlet (group) area is advantageous for the discharge of a curtain gas stream at ~e optimum curtain gas stream velocity, in suf~lcient volume to provide an effective gas curtain.
Preferred embodiments of ~e invention will now be described by way of example with reference to the accompanying drawings, in which:
Fig. 1 is a diagram of the spray zone on a subs~ate su~face during the implementation of the method oiF the invention;
Fig. 2 is a diagrarnmatic and partial section through a spray lance of the invention;
Fig. 3 is a dia~am o~ an erosion test conducted on refractory masses.

In Fig. 1, reference 1 represents a target portion of the surface of the substrate on which it is desired to form a refractory ceramic weld rnass by spraying this surface with a carrier gas stream comprising oxidizing gas and a mixture of refractory particles and fuel. This 5 carrier gas stream strikes the surface 1 in the diagram at an impact zone 2. According to the invention, the surface 1 is simultaneously sprayed with one or more peripheral gas jets which surround the impact zone 2 to form a gas curtain around the impact zone 2. Fig. 1 shows in diagrarnmatic forrn the intersection of this gas curtain with the surface 1 0 at an annular zone 3 which closely surrounds the impact zone 2. It is evident that the annular zone 3 may in practice be slightly spaced from ~he impact zone 2 or in contrast that the annular zone 3 and the impact zone 2 may partially interpenetrate one another.
In Fig. 2, the spray head 4 of the lance S comprises a central outlet 5 6 ~or spraying the carrier gas stream 7 comprising the mixture of particles dispersed in the oxidizing gas. In place of a single central outlet 6, the lance may comprise a group of several outlets for spraying the carrier gas stream 7. A spray lance comprising a outlet group of this type is disclosed and claimed for instance in Glaverbel's British ~o Patent Specification 2,170,122. The lance head 4 also comprises, in accordance with the invention, curtain gas spray means. In the embod~ment shown in Fig. 2, the curtain gas spray means comprise an annular outlet 8 which surrounds and is spaced from the central ou~let 6 in order to spray a substantially continuous annular gas stream 9. The 25 gas stream 9 fo~ns the gas curtain 3' which strikes the surface 1 in an annular zone 3. In a specific example, the area of the almular outlet is slightly more than double the area of the central outlet 6. The mixture of particles, dispersed in the oxidizing gas, is in~oduced via the supply tube 10 and the gas of the curtain gas jet Yia the duct 11. The 30 lance 5 also comprises an external cooling ring 12 d~

with a cooling water inlet and outlet. Fig. 2 also shows a cooling ring 13, with a cooling water inlet and outlet, which keeps the annular outlet 8 spaced from the central outlet 6. This cooling ring may be omitted, however, if so desired and replaced by a single small insert making it s possible to keep the annular outlet 8 spaced from the central outlet 6, -for example by 7mrn.
Fig. 3 is a diagram of an erosion test on a refractory ceramic weld mass. A prismatic bar 14, cut from the refractory mass to be tested, is partially immersed in a molten glass bath 15 at 1550C contained in a crucible (not shown~. This temperature is higher than the highest temperature normally used for molten soda-lime glass (ordinary window glass) in a glass melting furnace. The bar is kept immersed and its degree of wear examined after 16 hours.
Example 1 The ta~k blocks of the melting end of a glass melting furnace have to be repaired without cooling the furnace. These blocks are highly eroded, essentially at the location of the surface of the molten glass bath where "flux line corrosion" has taken place. l~hese tank blocks are highly refractory electrofused bricks based on alumina and zirconia, whose composi~ion comprises, by weight, 50-51% of alumina, 32-33%
of zirconia, 15-16% cf silica and approximately 1% of sodium oxide and which have a true density of 3.84. In order to permit access to this surface for repair, the level of molten glass was lowered by twenty or so centimetres. In order to carly out the repair, a carrier gas stream 2s comprising oxidizing gas and a mixture of refractory particles and fuel was sprayed onto the hot tank block. l'he mixt~e of particles comp~ised 40-50% of ZrO 2~ 38-44% of A1203, g 12% fuel made up of 8-4% of Al and 4-8% of Si, all by weight of the total mixt~re. The silicon particles were grairls with an average size of 6 ,Lm and a specific surface area of 5000 cm 2/g. The aluminium particles were grains wi~ an average size of S llm and a specific surface area of 4700 cm 2/g The maximum grain size of the alumirlium and silicon particles did not exceed S0 ~n. The silicon and alurninium particles combusted giving off sufficient heat to melt the refractory particles at least partially so that they bonded together. The 5 refractory particles of zirconia had an average grain size of lS0 llm and the refractory particles of alumina had an average grain size of lO0 llm.
In order to test the resistance to corrosion by glass of the refractory mass formed on the surface of the furnace tank blocks, a 0 re~ractory mass was firstly formed on the surface of a spare tank block heated to 1500C in a test f~unace using the method of the invention.
For ~is test, use was made of 8% by weight of Si and 4% by weight of Al in the mixture.
The mixture of particles dispersed in the oxidizing gas was 15 sprayed by the lance S shown in Fig. 2. It was introduced via the supply tube lO. The central powder outlet 6 was circular and had an area of l 13 mm2. The mixture was sprayed at a flow rate of 30 kg~
with oxygen as the oxidizing gas at a rate of 25 Nm 3~. The carrier gas stream 7 comprising the particle mixture and the oxidizing gas 20 struck the surface 1 to be treated at an impact zone 2. According to the invention this surface l was also sprayed with a curtain gas jet which formed a gas curtain 3' around the impact zone 2. In this example, the curtain gas jet was forrned by pure oxygen sprayed through the annular outlet 8 at a flow rate of 40 Nm 3/h in the forrn of an annular gas 25 stream 9 surro~ding the carrier gas stream 7 along its path from the head 4 of the lance 5 to the impact zone 2. The annular outlet 8 had a circular cross-section and an area of 310 mm 2. The annular outlet 8 was spaced ~rom the powder outlet 6 by 13 mm.

5,-During the implementatioll of the method, tne gas curtain 3' provided a supplementary means of acting on the evolution on the ceramic welding reaction and the formation of the refractory mass.
The ceramic welding reaction was stable and relatively well defined.
s The true porosi7ty of the mass ~olmed was 9% and its apparent porosity 1.5%. As the expressions are used in this specification, "apparent porosity" is measured by a method analogous to immersion and thus only takes account of open pores in the refractory material: "true porosity" also takes account of any closed pores in t7he refractory 10 material. The apparent density of the refractory mass formed, i.e. the density of the mass wi7~h its pores was 3.5. The true or absolute density of this mass7 i.e. the density of the refractory matrix material itself, measured on a sample finely crushed to eliminate ~e influence of the pores, was 3.85.
A prismatic bar 14 (Fig. 3) of 20 x 20 x 120 mm was cut from this refractory ceramic weld mass. This test bar was kept partially immersed in a bath lS of molten glass at 1550C contained in a crucible (not shown). The degree of wear of the bar after 16 hours was noted.
By way of comparison, a control sample of identical size was prepared and was kept partially immersed in the same molten glass bath at the same temperature. In order to facilitate the comparison, drawings of the control sample and the test bar have been showrl superimposed in Fig. 3. The control sarnple was a prisma~c bar which was cu~ from a refractory mass formed in the same way as the 2s refractory mass of Example 1 except that the curtain gas jet was omitted, i.e. a refractory ceramic weld mass formed by a method outside the scope of the present invention. The refractory mass folmed in this way had a ~ue porosity of 19.7% and an apparent porosity of 3.5%. It had an apparen~ density of 3.03 and an absolute density of 3.77.

~ ~ ~g '~

After 16 hours the bar 14 of the control sample assumed a shape shown diagran~natically by the dashed line 16. It can be seen that the imrnersed portion 17 of the bar 14 had undergone considerable colrosion as a result of its immersion in the glass bath. The edges of s the prism were rounded. It can be seen that the surface 18 of the molten glass bath 15 had considerably eroded the sample giving it a particular "flux line corrosion" shape at the zone indicated by reference numeral 19. The diameter of the bar at the centre of the "flux line corrosion" had been reduced to approximately one-third of its nominal lo value.
The bar 14 cut from the refractory mass formed by the implementation of the method of the invention assumed, after 16 hours, the shape shown by the dashed line 20. The erosion of the immersed portion was obviously smaller. The edges of the prism had not been 15 rounded to any great extent. The "flux line corrosion" 19 was far less pronounced than in the control sample. The diameter of the bar at the centre of the "flux line corrosion" was reduced to only approximately two-thirds of its nominal value. The use of the method of the invention thus enabled the production of a re~ractory mass much more resistant to 20 erosion than the mass foImed by the prior method. Microscope exarnination of a section of the bar also showed that there were in practic¢ no residual metal phases showing that the oxidation of the metal particles was in practice complete. This factor is very favourable for a refractory mass which has to come into contact with molten glass 25 as it is known ~at the contact of metal phases with the molten glass may cause bubbles to develop in the glass.

~mple 2 As a variant of Fig. 1, a refractory ceramic weld mass was produced in ~e same way as in Example l except that the oxygen flow rate of the carrier gas stream 7 was 30 Nm 3/h and tne oxygen flow rate of the curtain gas jet 9 was 20 Nm 3/h. The refractory cerarnic weld mass formed had an apparent porosity of 2%, a true porosity of 8.3%, an apparent density of 3.56 and a true density of 3.88.
A prismatic bar 14 was cut from this cerarnic weld mass and partially immersed in the molten glass bath 15 contained in the o crucible. After 16 hours the erosion test showed erosion similar to tne ceramic weld mass of Example l. The bar assumed the shape shown by the dashed line 20. Microscope examina~ion of a section of this bar also showed that there were in practice no residual metal phases.
Example 3 A refractory ceramic weld mass was produced in the same way as in Exarnple l except that the curtain gas jet 9 was formed by carbon dioxide sprayed at a flow rate of 20 Nm 3/h and the oxygen of thç
carrier gas stream 7 was sprayed at a flow rate of 30 Nm 3/h. It was also observed that ~e cerarnic welding reaction was stable and relatively well defined. l'he refractory ceramic weld mass formed had an apparent porosi~ of 1.5%, a true porosity of 4.6%, an apparent density of 3.5 and an absolute density of 3.67.
A prismatic bar 14 was cut from this ceramic weld mass and partially immersed in the molten glass bath 15 contained in the 2s crucible. ~fter 16 hours the erosion test showed erosion s~milar ~o the ceramic weld mass of Example l. The bar substantially assumed the shape shown by the dashed line 20.

"~ ri d~

E~ample 4 A refractory ceramic weld mass was produced in the same way as in Example 1 except that the gas curtain 9 was formed by nitrogen sprayed at a flow rate of 18 Nm 3/h and the oxygen of the carries gas stream 7 was sprayed at a flow rate of 30 Nm 3/h. It was also observed that the cera~r.ùc welding reaction was stable and relatively well defined. The refractory ceramic weld mass formed had an apparent porosity of 2.5%, an apparent density of 3.5 and a true density of 3.69.
o A prismatic bar 14 was cut from this ceramic weld mass and partially immersed in the molten glass bath lS contained in the crucible. ~fter 16 hours the erosion test showed erosion similar to the ceramic weld mass of Example 1. The bar substantially assumed the shape shown by the dashed line 20.
Exa~mple 5 The following mixturç, by weight, was used to carry out a consolidation repair to a fumace vault formed by silica bricks at a temperature of approximately 1500C: ~7% of refractory silica particles, 12% of combustible silicon particles and l~o of combus~ible aluminium particles. The silicon and aluminium particles each had an average grain size of less ~an 10 ~Lm, the specific surface area of the silicon being 4000 cm /g and that of the aluminium 6000 cm /g.
The maxi~um grain size of the alumil~ium and silicon par~icles did not exceed 50 ~n.
This mixture was sprayed using the method of the invention. The particle mixture was introduced with pure oxygen via the supply h~be 10 at a rate of 35 kg/h of material and 25 Nm 3/h of oxygen for spraying in the form of the carrier gas s~eam 7. In accordance with the invention, the target surface 1 to be treated was also sprayed with a curtain gas jet which fo~ned a gas curtain 3' around ~he impact zone 2. In this example, the curtain gas jet was ~ormed by pure oxygen sprayed at a flow rate of 30 Nm 3/h in the form of a curtain gas jet 9 r i ~ ,~ -f ~ ~ 4;

sulTounding the carrier gas stream 7 along its path from the head 4 of the lance 5 to the ~npact zone 2. No non-combusted metal was in practice found in the ceramic weld mass formed.
By way of comparison, a refractory ceramic weld mass was 5 formed by spraying ~he same mixture as above at a rate of 30 kg/h with a same oxygen flow rate of 25 Nm 3/h. For this comparison, however, the curtain jet of oxygen was omitted.
During the implementation of the method of the invention, it was observed that the gas curtain 3' provided a supplementary means of o action for controlling the formation of the refractory ceramic weld mass which did not exist in ~e case of the companson test. Moreover, the gas curtain 3' isolated the impact zone 2 so that the atrnospheric turbulence due to the operation of the furnace during the repair had practically no effect on the forrnation of the refractory ceramic weld -5 mass. The ceramic welding reaction was more stable and better confined and did not take place interm~ttently.
Example 6 A copper converter used in the non-ferrous metals industry was to be repaired~ The same method as in Example 5 was used except that 20 the mixture had the following composition by weight: 40% of chromium oxide particles, 48% of magnesium par~icles and 12% of aluminium particles. The aluminium particles had a nominal maximum grain size of 45 ~lm and a specific surface area of more than 3000 cm /g. The refractory particles all had a maximum size of less 2~ ~an 2 rnm. This example also showed that, as a result of the implementation of the invention, the gas curtain provided a supplementary means of action for con~oll~ng the evolution of the ceramic welding reaction and the formation of the reiractory cerarnic weld mass. 'l he cerarnic welding reaction was stable and well confmed.

By way of a variant, the annular outlet 8 of the spray head 4 was replaced by a series of injectors spraying gas jets converging to forrn the gas curtain 37. Very good results were also obtained with this spray lance.
Example 7 It was desired to form a refractory ceramic weld mass having a composition as close as possible to the basic refractory on a wall of a steelworks converter formed by magnesium-carbon bricks comprising 90% by weight of magnesia and 10% of carbon. The wall was at a o temperature of 900C. These bricks were sprayed with a par~icle mixture compnsing particles containing carbon. The mixture was sprayed at a rate of 500 kg~our in an oxidizing gas carrier gas s~eam containing 70% by volume of oxygen. The mixture had the following composi~ion by weight:
MgO 82%
Si 4%
Al 4%
C 10%.
the silicon particles had an average diameter of 10 ~Lm and a specific surface area of 5000 cm 2/g. 'rhe aluminium particles had an average diameter of 10 ~un and a speciflc surface area of 8000 cm 2/g T~e carbon particles were particles formed by crushing coke and their average diameter was 1.25 mm. The magnesia particles had an average diameter of 1 rnm. According to the invention, a gas curtain was formed around the impact zone of the carrier gas stream comprising the particles dispersed in the oxidizing gas on the wall of the converter by spraying carbon dioxide at a rate of flow 50% higher than the flow rate of the oxidizing gas to form a gas curtain around this carrier gas stream. It was observed during the implementation of the method ~at the ceramic welding reaction was stable and well J ~

confined. The carbon particles sprayed did not oxidize totally so that the ceramic weld mass formed contained some 5% of carbon. Without the gas curtain formed by the carbon dioxide jet the ceramic weld mass formed contained only some 3% of carbon.

In a variant embodiment of lance for the discharge of ceramic welding powder at a rate of between 900 kg/h and 1,000 kg/h, there is a cen~al powder discharge outlet 6 having a diameter of 53 mm and thus an area of 2,206 mm2. The lance also comprised a continuous annular curtain gas discharge outlet having an area of 1,979 mm 2 0 spaced frsm the powder discharge outlet by 13 mm, for example by means of a sleeve adapted on the end of the cen~al pipe or by means of a cooling ring 13. The lance also comprised an external cooling ling 12.

Claims (20)

1. A ceramic welding process in which a ceramic welding powder comprising a mixture of refractory particles and particles of a fuel material which is capable of being oxidized to form a refractory oxide is projected against a surface in one or more streams of carrier gas which contains at least sufficient oxygen for substantially complete oxidation of the fuel particles, whereby sufficient heat is released for at least surface melting of the projected refractory particles and a ceramic weld mass is formed against said surface under the heat of oxidation of the fuel particles, characterised in that at least one additional stream of gas is projected against said surface so as to form a substantially continuous gas curtain surrounding said carrier gas stream(s).
2. A process according to claim 1, wherein the gas curtain is projected as an annular stream.
3. A process according to claim 1 or 2, wherein the carrier gas is ejected from an outlet having an area of between 50 and 500 mm2 and the gas curtain is ejected from one or more outlets spaced from the carrier gas outlet by a distance of between 5 and 20 mm.
4. A process according to claim 1 or 2, wherein the carrier gas is ejected from an outlet having an area of between 300 and 2,300 mm and the gas curtain is ejected from one or more outlets spaced from the carrier gas outlet by a distance of between 10 and 30mm.
5. A process according to any preceding claim, wherein the volume rate of discharge of the curtain gas is at least half the volume rate of discharge of the carrier gas.
6. A process according to any preceding claim, wherein the discharge velocity (calculated at normal pressure) of the curtain gas is greater than one fifth of the discharge velocity of the carrier gas.
7. A process according to claim 6, wherein the discharge velocity (calculated at normal pressure) of the curtain gas is between one fifth and three fifths of the discharge velocity of the carrier gas.
8. A process according to any preceding claim, wherein the gas streams are discharged from a lance which is cooled by fluid circulating through it.
9. A process according to any preceding claim, wherein the curtain gas comprises oxygen.
10. A process according to any of claims 1 to 8, wherein the particles discharged in the carrier gas stream include particles of an oxidizable material which is to be incorporated as such in the weld mass and the curtain stream is substantially free from available oxygen.
11. A process according to any preceding claim, wherein the fuel material comprises one or more of materials in the group consisting of:
aluminium, silicon, magnesium, zirconium and chromium.
12. A process according to any preceding claim, wherein at least 50% by weight of the fuel particles have a grain size less than 50µm.
13. A process according to any preceding claim, wherein at least the greater part by weight of the refractory particles projected consists of alumina and/or zirconia or of magnesia and/or alumina.
14. A ceramic weld mass formed by a process according to any of claims l to 13.
15. A lance comprising an outlet for the discharge of a ceramic welding powder in a carrier gas along a discharge path towards a surface for the performance of a ceramic welding process, characterised in that such lance comprises a second outlet or group of second outlets, for the discharge of gas, said second outlet or outlet group being so shaped and arranged and so spaced both axially and radially in relation to the powder outlet that gas can be discharged from said second outlet or outlet group so as to form a substantially continuous curtain surrounding and generally parallel to the powder discharge path.
16. A lance according to claim 15, wherein such second outlet is a continuous annular outlet.
17. A lance according to claim 15 or 16, wherein such powder outlet has an area of between 50 and 500 mm2 and the or each said second outlet is spaced from the powder outlet by a distance of between 5 and 20 mm.
18. A lance according to claim 15 or 16, wherein such powder outlet has an area of between 300 and 2,300 mm2 and the or each said second outlet is spaced from the powder outlet by a distance of between 10 and 30 mm.
19. A lance according to any of claims 15 to 18, wherein such lance incorporates a jacket adapted for the circulation of coolant.
20. A lance according to any of claims 15 to 19, wherein the area of the second outlet is between two thirds of and three times the area of the powder outlet.
CA002026944A 1989-10-05 1990-10-04 Ceramic welding process and lance for use in such process Abandoned CA2026944A1 (en)