CA2459111C - Direct addition of beta-aminoenones in organic electrolytes of nonaqueous cells employing solid cathodes - Google Patents

Direct addition of beta-aminoenones in organic electrolytes of nonaqueous cells employing solid cathodes Download PDF

Info

Publication number
CA2459111C
CA2459111C CA2459111A CA2459111A CA2459111C CA 2459111 C CA2459111 C CA 2459111C CA 2459111 A CA2459111 A CA 2459111A CA 2459111 A CA2459111 A CA 2459111A CA 2459111 C CA2459111 C CA 2459111C
Authority
CA
Canada
Prior art keywords
alloys
cathode
electrolyte
lithium
additive
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CA2459111A
Other languages
French (fr)
Other versions
CA2459111A1 (en
Inventor
Andrew Webber
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Edgewell Personal Care Brands LLC
Original Assignee
Eveready Battery Co Inc
Energizer Brands LLC
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Eveready Battery Co Inc, Energizer Brands LLC filed Critical Eveready Battery Co Inc
Publication of CA2459111A1 publication Critical patent/CA2459111A1/en
Application granted granted Critical
Publication of CA2459111C publication Critical patent/CA2459111C/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

A method for manufacturing a nonaqueous cell employing an anode, a cathode and an organic electrolyte wherein the cathode comprises an active cathode material, and the organic electrolyte contains a beta-aminoenone in a range of 0.1 to 5.0 volume percent based on the volume of the electrolyte solvent so as to aid in reducing the undesirably high initial open circuit voltage normally observed with the use of cathodes such as FeS2.

Description

DIRECT ADDITION OF BETA-AIVIINOENONES IN ORGANIC
ELECTROLYTES OF NONAQUEOUS CELLS EMPLOYING SOLID
CATHODES
DESCRIPTION
Technical Field The invention relates to a method for manufacturing a nonaqueous cell employing an anode, a cathode comprising an active cathode material and an organic electrolyte. The method involves the direct addition of an additive such as beta-aminoenone, preferably 4-amino-3-penten-
2-one, to the electrolyte to aid in reducing any undesirably high initial open circuit voltage such as that normally observed with cathodes such as FeS2.
Background Art The development of high energy cell systems requires the compatibility of an electrolyte possessing desirable electrochemical properties with highly active anode materials, such as lithium, calcium, sodium and the like, and the efficient use of high energy density cathode materials. Such suitable high energy density cathode materials includes iron sulfides such as FeS2 and FeS, carbon flourides such as CF,-, metal oxides such as V205, W03, M003, lead oxides such as Pb304, Pb02 and Pb0, cobalt oxides such as Co304, manganese oxides such as Mn02, In2S3, NiS, metal chromates such as Ag2Cr04, metal phosphates such as Ag3PO4, LiCo02, LiMn204, Bi,03, CuO and Cu20 and metal sulfates such as CuSO4. The use of aqueous electrolytes is precluded in these systems since the anode materials are sufficiently active to react with water chemically.
Therefore, in order to realize the high energy density obtainable through use of these highly reactive anodes and high energy density cathodes, it is necessary to use a nonaqueous electrolyte system.

Many cell or battery applications, particularly in transistorized devices, such as hearing aids, watches, calculators, and the like, require a substantially unipotential discharge source for proper operation. However, it has been found that in many nonaqueous cells employing positive active materials, which include conductive additives such as graphite andJor carbon, the cell upon initially being discharged, exhibits a high voltage whereupon the cell then proceeds to reach its lower operating discharge voltage level only after a certain time period has elapsed. The time period for the cell to reach its intended operating discharge voltage level usually depends on the discharge rate through the load and thus, depending on the apparatus it is to power, could result in a period extending up to several hours or .even days. This phenomenon has serious Ch-awbacks when a cell is intended to be used in electronic devices requiring a substantially unipotential discharge source for proper operation. In some of these electronic devices, any initial voltage peak substantially exceeding the intended operating voltage for the device could result in serious damage to the electronic components of the device.
One approach to protect devices from batteries exhibiting high voltages prior to leveling off to their desired operating voltage level is to add additional electronic circuit components to protect the main operating components of the device. However, this not only adds to the expense of the device but also would result in enlarging the device to accommodate the protective circuitry. Larger devices run counter to the current emphasis placed on miniaturization, where it has become necessary for the battery industry to design smaller and smaller electrochemically powered cells.
Another approach designed to reduce an initially high and potentially disadvantageous voltage is to subject such cells to a pre-discharge regimen prior to initial use by an end user. - But such pre-discharge regimens are time consuming and costly, and reduce the capacity of the cell. Therefore, it is desirable to reduce or eliminate any required pre-discharge.
It has been suggested in U.S. Pat. No. 4489144 that the addition of an isoxazole derivative, such as 3,5-dimethylisoxazole, to the electrolyte may compensate for or eliminate this initial high voltage during discharge of nonaqueous cells. It was believed that the isoxazole derivative reacted with unwanted species that presumably caused the initial high voltage by reducing these species. The entire disclosure of U.S. Pat. No.
4489144 may be referred to for further details.
It has now been determined that a favorable reduction in initial open circuit voltage in a nonaqueous cell can be achieved by the addition of an additive as defined below to the electrolyte. Accordingly, it is an aspect of the within invention to provide a method for manufacturing a cell comprising a highly active anode such as lithium, a cathode comprising an active material such as FeS2, and a nonaqueous electrolyte comprising an additive, such as 4-amino-3-penten-2-one.
In a broad aspect the invention comprehends a method for manufacturing a nonaqueous cell comprising the steps of providing an anode, an organic electrolyte solution comprising a solute dissolved in an organic solvent, and a solid cathode, and adding an additive to the electrolyte solution, the additive added to the electrolyte solution in a range of 0.1 to 5.0 volume percent based on the volume of the organic solvent and defined as any one of:
-CO-CR=C(N112)-where R is hydrogen or an alkyl group; or -CO-CR=C(NR2R 3) where R, R2 and R3 are hydrogen or an alkyl group; or related azirenes of the formula -CO-CRR'-C(NR2R3)(R")-where R, R', R", R2 and R3 are hydrogen or an alkyl group.
3 Detailed Description Of The Invention The addition of the additive, such as 4-amino-3-penten-2-one, to nonaqueous organic electrolytes is effective in reducing and stabilizing the undesirably high initial open circuit voltages observed with cathode materials such as FeS2. As used herein, the term "additive"
will be used to describe a material containing any of the above structures.
A preferred additive is a beta-aminoenone such as 4-amino-3-penten-2-one.
The additive is preferably employed in the concentration range of between 0.1 and 5.0 volume percent based on the volume of the electrolyte solvent, preferably between 0.2 and 4.0 volume percent, and still more preferably between 0.2 and 2.0 volume percent, for most nonaqueous electrochemical couples.
The effectiveness of such additive in controlling initially high open circuit voltage was first discovered while examining the electrolyte solution of nonaqueous cells employing carbon and/or graphite-containing FeS2 cathodes and lithium anodes. These cells were manufactured with an electrolyte solvent that included 3,5-dimethylisoxazole (DMI), an isoxazole derivative, as described in U.S. Pat. No. 4489144. Upon aging, gas chromatography (GC) studies on the electrolyte from the undischarged cells revealed that the DMI was no longer detectable.
Instead, an amine was detected which was not initially present in the electrolyte. The amine was identified as 4-amino-3-penten-2-one (AP), one member of a class of beta-aminoenones.
A second compound was also detected which was not initially present in the electrolyte: 2,4-pentanedione (PD). It is believed that the presence of PD is at least in part an artifact produced by exposure of the electrolyte to water during the GC sample preparation.
4 The reaction mechanism involving DMI and AP was further investigated by GC
analysis of electrolytes from vial storage studies. In these studies, various components of a Li/FeS2 cell were isolated and combined with electrolyte containing DMI. The procedure in general was as follows: A 3/4 inch square piece of cell component sample was placed in a 1 ounce jar. An electrolyte was prepared containing 1 mole of LiCF3S03 added to 1 liter of 25:75:0.2 DIOX:DME:DMI by volume, where DIOX is 1,3-clioxolane and DME is 1,2-dimethoxyethane. One hundred micro liters of electrolyte was added to a vial.
The vial was then capped and stored in the dry box for three hours. At the end of this period, the electrolyte was recovered in methylene chloride, the solution was extracted with water and the methylene chloride layer was analyzed.
Initially, electrolyte reaction with the lithium, separator material and cathode stock was examined. The results are presented in Table 1.
TABLE 1:
PERCENT OR PPM BY GC PEAK AREA
REACTANTS % DIOX % DME % DMI ppm AP
Electrolyte + 23.42 76.14 .44 ND*
lithium foil Electrolyte + 23.66 75.91 .44 ND*
separator Electrolyte + 21.97 77.87 .09 614 cathode stock Electrolyte 25.48 74.14 .38 ND*
*None detected.
The above data indicate that DMI is degraded in a reaction involving the cathode. To further isolate the point of DMI degradation, cathode mix was isolated from the aluminum foil substrate and the vial test was run on the cathode mix and this aluminum separately.
The mix and the aluminum substrate were recombined and another vial test was run. A

further vial test was run on cathode mix and fresh aluminum. The results are presented in Table 2.
TABLE 2:
PERCENT OR PPM BY GC PEAK AREA
REACTANTS % DIOX % DME % DMI ppm AP ppm PD
Electrolyte + 23.88 75.52 .44 ND* ND*
cathode mix Electrolyte + 24.04 75.46 .43 ND* ND*
alum. substrate Electrolyte + 23.61 76.06 .25 362 534 cathode mix +
alum. substrate Electrolyte + 24.18 75.45 .31 47 477 cathode mix +
fresh aluminum *None detected.
In a further attempt to isolate the reactive species in the degradation of DMI
and the generation of AP, cathode mix components were individually subjected to the vial test in combination with fresh substrate aluminum. These results are presented in Table 3.
TABLE 3:
PERCENT OR PPM BY GC PEAK AREA
REACTANTS % DIOX % DME % DMI ppm AP ppm PD
Electrolyte + FeS2 20.27 78.90 .42 ND* ND*
(undried) Electrolyte + Acetylene 25.24 74.38 .38 ND* ND*
black Electrolyte + polyethylene 25.32 74.27 .41 ND* ND*
/polypropylene copolymer Electrolyte + polyethylene 25.13 74.47 .38 ND* ND*
oxide *None detected.

The above data indicates that the DMI degradation reaction to produce AP only takes place in the presence of both the cathode mix and an aluminum substrate current carrier, and suggests that the degradation reaction involves a possible interaction of the cathode mix with the aluminum cathode current carrier.
Further experiments were carried out to determine whether the direct addition of AP
or PD into the electrolyte solvent in place of DMI would show similar advantageous results in reducing the open circuit voltage of an undischarged cell. Several lots of nonaqueous AA
size lithium anode iron pyrite cathode cells were constructed using the electrolyte described above with the following variations: a) no DMI, b) 0.2% DMI, c) 0.2% PD
(instead of DMI) and d) 0.2% AP (instead of DMI), all by volume percent of the electrolyte solvent.
The pyrite for these cells came from different production batches as indicated in the attached tables but was essentially the same material. The cells were stored either at ambient temperature (21 C) or at 60 C. The cells were removed from storage at the indicated period in the tables below and the open circuit voltage for the cell was measured.
The cells were then autopsied and GC analysis was performed on the electrolyte. The results for the ambient cells are presented in Table 4 and for the 60 C cells in Table 5.
Significantly, none of these cells contained any detectable amounts of DMI even after only two weeks at ambient temperature, indicating that the degradation reaction is completed relatively quickly, even at ambient storage temperatures.
TABLE 4: STORAGE AT 21 C
Electrolyte description/ Pyrite lot # OCV prior to ppm AP (by GC ppm PD (by GC
storage duration autopsy (Volts) peak area) peak area) No DMI 171 2 weeks 1.727 ND* ND*
7 weeks 1.757 ND* ND*
23 weeks 1.785 ND* ND*
No DMI 172 Electrolyte description/ Pyrite lot # OCV prior to ppm AP (by GC ppm PD (by GC
storage duration autopsy (Volts) peak area) peak area) 2 weeks 1.732 ND* ND*
10 weeks 1.760 ND* ND*
16 weeks 1.775 ND* ND*
0.2% DMI 171 2 weeks 1.725 1441 ND*
7 weeks 1.748 334 ND*
, 23 weeks 1.748 ND* ND*
0.2%DMI 172 2 weeks 1.726 1080 ND*
10 weeks 1.730 51 ND*
16 weeks 1.745 32 ND*
0.2%PD 171 2 weeks 1.725 ND* 39 7 weeks 1.758 ND* ND*
23 weeks 1.780 ND* ND*
0.2%AP (supplied by 172 Lancaster Synthesis) 2 weeks 1.727 1379 ND*
10 weeks 1.730 ND* ND*
16 weeks 1.740 304 ND*
0.2%AP (supplied by 172 TCI) 2 weeks 1.727 2215 ND*
10 weeks 1.740 192 ND*
16 weeks 1.740 ND* ND*
*None detected.
TABLE 5: STORAGE AT 60 C
Electrolyte description/ Pyrite lot # OCV PRIOR ppm AP
(by GC ppm PD (by GC
storage duration TO AUTOPSY peak area) peak area) (Volts) No DMI 171 4 weeks 1.846 ND* ND*
12 weeks 1.847 ND* ND*
No DMI 172 4 weeks 1.830 ND* ND*
12 weeks 1.830 ND* ND*
.2% DMI 171 4 weeks 1.798 ND* ND*
12 weeks 1.837 ND* ND*
' .2%DMI 172 4 weeks 1.810 ND* ND*
12 weeks 1.824 ND* ND*
.2%PD 171 ' =
Electrolyte description/ Pyrite lot # OCV PRIOR ppm AP (by GC ppm PD (by GC
storage duration TO AUTOPSY peak area) peak area) (Volts) 4 weeks 1.840 ND* 32 12 weeks 1.834 ND* ND*
.2%AP (supplied by 172 Lancaster Synthesis) 4 weeks 1.810 ND* ND*
12 weeks 1.750 ND* ND*
.2%AP (supplied by 172 TCI) 4 weeks 1.760 267 ND*
12 weeks 1.790 ND* ND*
*None detected A study of the open circuit voltages for the cells in Table 4 reveals the following: at 16 weeks ambient, the cells with DMI in the electrolyte have a 30 mV lower open circuit voltage than the cells without DMI, confirming the observation disclosed in US
Pat. No.
=
4489144 that DMI aids in reducing undesirably high open circuit voltage in such cells. The cells containing AP have a 35 mV lower open circuit voltage than the cells with no DMI.
On the other hand, at 23 weeks ambient there is a 37 mV difference between the DMI cells and the no added DMI cells, but only a 5 mV difference between the PD cells and the cells without DMI. In general, it can be concluded that the cells with AP added to the electrolyte behave in the same manner as do cells with added DMI in reducing open circuit voltage, while the cells with PD added to the electrolyte behave in the same manner as do cells without any DMI added to the electrolyte. The cells represented in Table 5 demonstrate that the addition of AP to the electrolyte reduces open circuit voltage.
Literature studies show that AP can be obtained by the partial reduction of DMI.
However, it is unexpected that DMI would be reduced in a reaction with the cathode, in view of the presence of an even stronger reducing agent, the lithium metal anode. However, when DMI is reduced with butyl lithium (often used to mimic the reducing power of lithium metal), the reaction product is 3-methyl-5-hydroxymethyl isoxazole, a compound that is not a beta-aminoenone as defined herein. The fact that this reaction product is not seen in the studies represented in Tables 1 through 5, together with the fact that AP does react readily with lithium metal, further supports the proposition that DMI is reduced in a reaction with the cathode to lower the cathode voltage and the resulting AP is consumed by the lithium anode. Based on this information, it would not be expected that AP would react with the cathode to lower its voltage. Lowering the cathode voltage presumably involves reducing the cathode. Thus, the more reducing power the additive has the more likely it is to lower the cathode voltage. AP, on the other hand, is a reduced form of DIVII in that AP has two additional hydrogen atoms. AP, being already partly reduced, has less reducing power than DML Consequently, one would not have expected AP to be as effective as DM1 or even effective at all in lowering the cathode voltage. However, the results in Tables 1 through 5 demonstrate that AP behaves in the same manner as does D1\4I and does lower the cathode voltage.
The amount of the additive below 0.1 volume percent based on the volume of the electrolyte solvent would likely not provide sufficient feducing material to quickly and effectively reduce impurities and/or unwanted active species in the cell system. An amount above 5.0 volume percent based on the volume of the electrolyte solvent may provide excessive reducing material)that could cause deleterious effects on other desired aspects of the cell. Although one embodiment of the invention, if focusing solely on voltage reduction, would include the use in the cathode of a metallic reducing agent such as zinc in conjunction with the additive in the electrolyte, the additive can be used without the metallic reducing agent in the cell, without departing from the scope of the within invention. The omission of such a reducing agent may in fact be preferable, since such reducing agents may produce other undesirable features within the cell.
If the within invention is practiced in conjunction with the addition of a metallic reducing agent, the metallic reducing agent can either be employed in a mixture in the forming of a cathode or it could be placed in contact with the cathode. Thus, any discrete material such as a layer, a coating, a metallic screen, a metallic strip, a porous metallic strip, or a powder and could be employed as long as it is in electronic and ionic contact with the cathode. The choice of a metallic reducing agent will depend upon the voltage of the cell's active cathode material with reference to the anode of the cell. For example, while zinc may be satisfactory for a nonaqueous lithium/FeS2 system, it may not be suitable for a nonaqueous lithium/Ag90 system since, in the latter, a less anodic (negative) metallic reducing agent may be required, such as tin or lead. Thus, once the EMF series is determined for a specific nonaqueous electrolyte and anode/cathode system, one can select which metallic reducing agents can be used in conjunction with the additive.
In the nonaqueous cell systems of this invention, suitable active cathode materials would include iron sulfides such as FeS2 and FeS, carbon flourides such as CF, metal oxides such as V205, W03, Mo03, lead oxides such as P11304, Pb02 and Pb0, cobalt oxides such as Co304, manganese oxides such as Mn02, In2S3, NiS, metal chromates such as Ag2CrO4, metal phosphates such as Ag3PO4, LiCo02, UM:1204, B1203, CUO and Cu20 and metal sulfates such as CuSO4. Highly active anodes for use in nonaqueous systems according to this invention would be consumable metals and include aluminum, the alkali metals, alkaline earth metals and alloys of alkali metals or alkaline earth metals with each other and other metals. The term "alloys" as used herein is intended to include mixtures, solid solutions, such as lithium-magnesium, and the intermetallic compounds, such as lithium monoahaminide. The preferred anode materials are lithium, sodium, potassium, calcium, magnesium and alloys thereof. Carbon anodes such as are used in lithium ion cells are also suitable anodes for use with the present invention. A preferred anode material to be used in conjunction with an FeS2 cathode having an aluminum cathode substrate would be a lithium-aluminum alloy such as that disclosed in US Pat. No. 5514491, which may be referred to for further details. One such alloy is 0.5% aluminum by weight and is available from Chemetall-Foote.
In nonaqueous cells, useful organic solvents employed alone or mixed in the cell of this invention include the following classes of compounds: alkylene nitriles:
e.g., crotonitrile (liquid ranges, -51.1 to 120 C); trialkyl borates: e.g., trimethyl borate, (CH30)3B
(liquid range, -29.3 C to 67 C); tetraalkyl silicates: e.g., tetramethyl silicate, (CH30)4Si (boiling point, 121 C); nitroalkanes: e.g., nitromethane, CH3NO2 (liquid range, -17 C to 100.8 C); alkylnitriles: e.g., acetonitrile, CH3CN (liquid range, -45 C to 81.6 C);
dialkylamides: e.g., dimethylformamide, HCON(CH3)2 (liquid range, -60.48 C to 149 C);
lactams: e.g., N-methylpyrrolidone, (liquid range, -16 C to 202 C);
monocarboxylic acid esters: e.g., ethyl acetate (liquid range, -83.6 C to 77.06 C); orthoesters:
e.g., trimethylorthofoimate, HC(OCH3)3 (boiling point, 103 C); lactones: e.g., (gamma)butyrolactone, (liquid range, -42 C to 206 C); dialkyl carbonates:
e.g., dimethyl-carbonate, OC(OCH3)2 (liquid range, 2 C to 90 C); alkylene carbonates: e.g., propylene carbonate (liquid range, -48 C to 242 C), ethylene carbonate and vinylene carbonate;
monoethers: e.g., diethyl ether (liquid range, -116 C to 34.5 C); polyethers:
e.g., 1,1-and 1,2-dimethoxyethane (liquid ranges, -113.2 C to 64.5 C and -58 C to 83 C, respectively);
cyclic ethers: e.g., tetrahydpfuran (liquid range, -65 C to 67 C), 1,3-dioxolane (liquid range, -95 C to 78 C) and substituted dioxolanes; nifroaromatics: e.g., nitrobenzene (liquid range, 5.7 C to 210.8 C); cyclic sulfones: e.g., sulfolane, (melting point, 22 C), 3-methylsulfolane (melting point, -1 C); saturated heterocyclics: e.g., tetrahydrothiophene (liquid range, -96 C to 121 C); 3-methyl-2-oxazolidone (melting point, 15.9 C); five-membered unsaturated heterocyclics: e.g. 1-meth-ylpyrrole (boiling point, 114 C), 2,4-dimethylthiazole (boiling point, 144 C), and furan (liquid range, -85.65 C to 31.36 C);
dialkyl sulfoxides: e.g., dimethyl sulfoxide (liquid range, 18.4 C to 189 C);
dialkyl sulfates:
e.g., dimethylsulfate (liquid range, -31.75 C to 188.5 C); dialkyl sulfites:
e.g., dimethylsulfite (boiling point, 126 C); alkylene sulfites: e.g., ethylene glycol sulfite (liquid range, -11 C to 173 C); halogenated alkanes: e.g., methylene chloride (liquid range, -95 C
to 40 C); 1,3-dichloropropane (liquid range, -99.5 C to 120.4 C). Of the above, the preferred solvents are sulfolane; tetrahydrofuran; methyl-substituted tetrahydrofuran; 1,3-dioxolane; alkyl substituted 1,3-dioxolane; 3-methyl-2-oxazolidone; propylene or ethylene carbonate; (gamma)butyrolactone; ethylene glycol sulfite; dimethylsulfite;
dimethyl sulfoxide; and 1,1-, 1,2-dimethoxyethane and glymes. Of the preferred solvents, the best are 3-methyl-2-oxazolidone, propylene or ethylene carbonate, 1,2-dimethoxyethane and 1,3-dioxolane because they appear more chemically inert to battery components and have wide liquid ranges, and especially because they permit highly efficient utilization of the cathode materials.
The ionizing solute for use in the invention may be a simple or double salt or mixtures thereof, e.g., LiCF3S03 or LiC104 or LiI, which will produce an ionically conductive solution when dissolved in one or more solvents. Useful solutes include complexes of inorganic or organic Lewis acids and inorganic ionizable salts.
The only requirements for utility are that the salts, whether simple or complex, be compatible with the solvent or solvents being employed and that they yield a solution which is sufficiently ionically conductive. According to the Lewis or electronic concept of acids and bases, many substances, which contain no active hydrogen can act as acids or acceptors of electron doublets. The basic concept is set forth in the chemical literature (Journal of the Franklin Institute, Vol. 226, July/December 1938, pages 293-313 by G. N. Lewis). A
suggested reaction mechanism for the manner in which these complexes function in a solvent is described in detail in U.S. Pat. No. 3,542,602 wherein it is suggested that the complex or double salt formed between the Lewis acid and the ionizable salt yields an entity which is more stable than either of the components alone. Typical Lewis acids suitable for use in the present invention include aluminum fluoride, aluminum bromide, aluminum chloride, antimony pentachloride, zirconium tetrachloride, phosphorus pentachloride, boron fluoride, boron chloride and boron bromide. Ionizable salts useful in combination with the Lewis acids include lithium fluoride, lithium chloride, lithium bromide, lithium sulfide, sodium fluoride, sodium chloride, lithium bromide, potassium fluoride, potassium chloride and potassium bromide.
The within invention can be utilized in the manufacture of both primary and secondary nonaqueous cells in a wide variety of cell constructions, including but not limited to cylindrical wound cells, cylindrical bobbin cells, miniature button cells, cells with one or more planar electrodes arranged in a co-facial orientation or in a co-planar orientation and prismatic cells. Further, although the experiments were performed by adding AP
to the electrolyte, one of skill in the art will appreciate that the same result can be expected by the addition of AP to the cathode of the cell, without departing from the scope of the within invention.

Claims (11)

WHAT IS CLAIMED IS;
1. A method for manufacturing a nonaqueous cell comprising the steps of providing an anode, an organic electrolyte solution comprising a solute dissolved in an organic solvent, and a solid cathode, and adding an additive to the electrolyte solution, the additive added to the electrolyte solution in a range of 0.1 to 5.0 volume percent based on the volume of the organic solvent, wherein the additive is defined as anyone of the following formulas:
-CO-CR=C(NH2)-where R is hydrogen or an alkyl group; or -CO-CR=C(NR2R 3)-where R, R2 and R3 are hydrogen or an alkyl group; or -CO-CRR'-C(NR2R3)(R")-where R, R', R", R2 and R3 are hydrogen or an alkyl group.
2. The method of claim 1, wherin the additive is in a range of from 0.2 to 4.0 volume percent based on the volume of the organic solvent.
3. The method of claim 1, wherein the additive is 4-amino-3-penten-2-one.
4. The method of claim 1, wherein the cathode comprises a material selected from the group consisting of iron sulfides, carbon flourides, V2O5, WO3, MoO3, Pb3O4, PbO2, PbO, Co3O4, manganese oxides, In2S3, NiS, Ag2CrO4, Ag3PO4, LiCoO2, LiMn2O4, Bi2O3, CuO, Cu2O and CuSO4.
5. The method of claim 1, wherein the anode comprises a material selected from the group consisting of lithium, sodium, potassium, calcium, magnesium, carbon, alloys of lithium, alloys of sodium, alloys of potassium, alloys of calcium, alloys of magnesium and alloys of carbon.
6. The method of claim 4, wherein the anode comprises a material selected from the group consisting of lithium, sodium, potassium, calcium, magnesium, carbon, alloys of lithium, alloys of sodium, alloys of potassium, alloys of calcium, alloys of magnesium and alloys of carbon.
7. The method of claim 6, wherein the cathode comprises FeS2 and the anode comprises a lithium-aluminum alloy.
8. The method of claim 7, further comprising the step of adding a polyether to the electrolyte solution.
9. The method of claim 8, wherein said polyether is 1,2-dimethoxyethane.
10. The method of claim 7, further comprising the step of adding a cyclic ether to the electrolyte solution.
11. The method of claim 10, wherein said cyclic ether is 1,3-dioxolane.
CA2459111A 2001-10-01 2002-09-30 Direct addition of beta-aminoenones in organic electrolytes of nonaqueous cells employing solid cathodes Expired - Fee Related CA2459111C (en)