CN1318339C - Colour glass blue colouring pigment and its preparing process - Google Patents

Colour glass blue colouring pigment and its preparing process Download PDF

Info

Publication number
CN1318339C
CN1318339C CNB2004100235395A CN200410023539A CN1318339C CN 1318339 C CN1318339 C CN 1318339C CN B2004100235395 A CNB2004100235395 A CN B2004100235395A CN 200410023539 A CN200410023539 A CN 200410023539A CN 1318339 C CN1318339 C CN 1318339C
Authority
CN
China
Prior art keywords
preparation
coloring agent
pigment
fusing assistant
agent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CNB2004100235395A
Other languages
Chinese (zh)
Other versions
CN1640835A (en
Inventor
段海廷
吴向松
范文祥
江小林
苏文海
刘景柱
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dezhou Zhenhua Decoration Glass Co Ltd
Original Assignee
Dezhou Zhenhua Decoration Glass Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dezhou Zhenhua Decoration Glass Co Ltd filed Critical Dezhou Zhenhua Decoration Glass Co Ltd
Priority to CNB2004100235395A priority Critical patent/CN1318339C/en
Publication of CN1640835A publication Critical patent/CN1640835A/en
Application granted granted Critical
Publication of CN1318339C publication Critical patent/CN1318339C/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

The present invention relates to a colored glass coloring agent and preparation technology thereof. The colored glass colouring agent is prepared from main materials of plumbum and boron and auxiliary materials of zinc, chromium and lithium, and the preparation technology comprises the technical processes of fluxing agent preparation, glaze fusing powder preparation, coloring matter preparation, coloring agent preparation, etc. to obtain a granular colored glass blue coloring agent. By adopting the novel coloring agent, the quality of a product is stable, the defects of similar products that color channels and gas bubbles are easily generated are overcome, operation is convenient, the effect of the novel coloring agent is superior to that of the similar coloring agents, the production cost of the novel coloring agent is greatly reduced, and the novel coloring agent can replace imported products.

Description

Coloured glass blue colorant and preparation technology
Technical field
The present invention relates to a kind of glass coloring immunomodulator compounds and preparation method.
Background technology
Late 1960s, coloured glass begins to occur abroad, China began one's study the seventies, originally be in the road, to add Powdered pigment, dye melts is after stirring action, make itself and parent glass be mixed into the material of homogeneous, through the homogenizing postforming, yet this coloured glass is had to limited popularization.The first, when in glass metal, adding tinting material, can produce many difficulties, the second, glass metal is carried out second-heating detrimentally affect, and subject matter is reboil bubble to occur.U.S.'s import particulate state tinting material is used in the back, and this tinting material generally adopts the boracic prescription, though improvement is arranged, but still have unstable product quality, defectives such as look road, bubble, color lump very easily appear, and the product import, cost an arm and a leg, be badly in need of substitute products.
Summary of the invention
Cost an arm and a leg in order to overcome prior art, unstable product quality, effect is undesirable, defectives such as look road, bubble, color lump very easily occur, the invention provides a kind of new coloured glass tinting material and production technique.
New coloured glass blue colorant provided by the present invention adopts plumbous boron prescription, and adds zinc, chromium, lithium composition in prescription, and its chemical ingredients is as follows: SiO 215-17%; AI 2O 33-5%; PbO25-30%; B 2O 33-6%; CuO35-40%; Co 2O 30.2-0.5%; MnO 20.5-1%; Cr 2O 31-2%; R 2O10-18%; ZnO4-5%.
Above-mentioned compound can prepare by following method.
(a) preparation of fusing assistant: the fusing assistant proportioning raw materials is SiO 230-35%; AI 2O 36-10%; CaO0.5-2%; MgO0.1-1%; PbO45-50%; B 2O 34-8%; K 2O+Na 2O10-15%;
(b) preparation of melted glaze powder: fusing assistant is heated in crucible 1100-1200 ℃ by above-mentioned chemical constitution batching back and is founded, soak 40-60min, and through shrend, ball milling, drying, sieving obtains melted glaze powder.
(c) preparation of pigment, it is toner that blue light agent adopts copper, cobalt, its composition of raw materials: CuO70-80%; Co 2O 30.5-1%; MnO 22-5%; Cr 2O 33-5%; ZnO8-10%; Li 2CO 38-10%; B 2O 33-5%.Borax is earlier soluble in water, and powder adds behind all the other raw material blendings, mixes oven dry thoroughly, and ball milling sieves, and obtains pigment
(d) preparation of tinting material: fusing assistant and pigment by fusion in crucible after 2: 1 mixed, are injected the cold water hardening crack then, and dry back fragmentation is sieved, the blue particle agent.
Embodiment
The invention will be further described below in conjunction with embodiment
The preparation of the coloured glass blue colorant of indication of the present invention realizes by following processing method.
One, the preparation of fusing assistant
In order to adapt to the processing temperature of expecting the road and the chemical constitution and the chemical property of glass basestocks.Reduce PbO, B 2O 3Deng the volatile quantity of raw material, fusing assistant is selected following raw materials according proportioning: SiO for use 230-35%; AI 2O 33-5%; CaO0.5-2%; MgO0.1-1%; PbO45-50%; B 2O 34-8%; K 2O+Na 2O10-15%.
Two, the preparation of melted glaze powder
Fusing assistant is formed the batching back by its said ratio and found into vitreum in crucible, and glass melting temperature is about 1180 ℃, and top temperature keeps 45min, pours into then and carries out shrend in the water, the molten glaze ball milling after the shrend 28 hours.Sieve on the 80th is crossed in dry back, obtains powdered frit.
Three, the preparation of pigment
It is toner that blue colorant adopts copper, cobalt, its pigment raw material proportioning: CuO70-80%; Co 2O 30.5-1%; MnO 22-5%; Cr 2O 33-5%; ZnO8-10%; Li 2CO 38-10%; B 2O 33-5%.The raw materials used chemical pure raw material that all adopts of pigment requires steady quality, and borax is earlier soluble in water, and powder behind all the other raw material blendings is added, mixes thoroughly oven dry, and ball milling was crossed 280 mesh sieves about 25 hours, obtained pigment.
One, the preparation of tinting material
By after 2: 1 mixed, the cold water hardening crack is injected in fusion in crucible then with fusing assistant and pigment, broken 4 orders of crossing in dry back, and 10 mesh sieves, intermediate particle is the particulate state blue colorant, its main chemical compositions: SiO 215-17%; AI 2O 33-5%; PbO25-30%; B 2O 33-6%; CuO35-40%; Co 2O 30.2-0.5%; MnO 20.5-1%; Cr 2O 31-2%; R 2O10-18%; ZnO4-5%.

Claims (1)

1, a kind of coloured glass blue colorant is characterized in that this tinting material is to adopt the method for following step to prepare:
(a) the fusing assistant proportioning raw materials is counted SiO with percent by weight 230-35%; Al 2O 36-10%; CaO0.5-2%; MgO0.1-1%; PbO45-50%; B 2O 34-8%; K 2O+Na 2O10-15%;
(b) preparation of fusing assistant: above-mentioned fusing assistant raw material is placed crucible, and 1100-1200 ℃ of down heating 40-60 minute, again through shrend, ball milling, drying, sieving obtains described fusing assistant;
(c) pigment preparation, the pigment raw material proportioning is counted CuO70-80% with percent by weight; Co 2O 30.5-1%; MnO 22-5%; Cr 2O 33-5%; ZnO8-10%; Li 2CO 38-10%; B 2O 33-5%, earlier that borax is soluble in water, add all the other raw materials behind the mixing again, mix oven dry thoroughly, ball milling, sieving obtains described pigment;
(d) above-mentioned fusing assistant is mixed according to weight ratio with above-mentioned pigment at 2: 1, the cold water hardening crack is injected in fusion in crucible more then, and dry back fragmentation is sieved and obtained described coloured glass blue colorant.
CNB2004100235395A 2004-01-17 2004-01-17 Colour glass blue colouring pigment and its preparing process Expired - Fee Related CN1318339C (en)